{"content":[{"fname":"Processing","content":["Injection Moulding","Extrusion","Sheet Extrusion","Other Extrusion"],"cattype":"features","name":"Characteristics","pos":2,"type":"Feature"},{"fname":"Delivery form","content":["Pellets"],"cattype":"features","name":"","pos":3,"type":"Feature"},{"fname":"Additives","content":["Lubricants","Release agent"],"cattype":"features","name":"","pos":4,"type":"Feature"},{"fname":"Special characteristics","content":["Low emissions"],"cattype":"features","name":"","pos":5,"type":"Feature"},{"cattype":"product_txt","name":"Product Text","content":"<span class=\"smallfont\">Common features of Delrin\u00ae acetal resins include mechanical and physical properties such as high mechanical strength and rigidity, excellent fatigue and impact resistance, as well as resistance to moisture, gasoline, lubricants, solvents, and many other neutral chemicals. Delrin\u00ae acetal resins also have excellent dimensional stability and good electrical insulating characteristics. They are naturally resilient, self-lubricating, and available in a variety of colors and speciality grades. <br\/><br\/>Delrin\u00ae acetal resin typically is used in demanding applications in the automotive, domestic appliances, sports, industrial engineering, electronics, and consumer goods industries.<br\/><br\/><\/span><span class=\"bluebg\">Delrin\u00ae 100P is a high viscosity acetal homopolymer for use in easy-to-fill molds. Delrin\u00ae 100P provides a great combination of toughness and strength, improved processing thermal stability and productivity for injection moulding, and low VOC emissions.<\/span>","protectxt":"","pos":6,"type":"Text"},{"content":[{"id":830134,"category":"regulatory","subcategory":"","filename":"EHSprofile","description":"Regulatory Information Sheet (RIS)"},{"id":775,"category":"regulatory","subcategory":"","filename":"public\/regulatory\/REACH__SVHC%20declaration_June%202025.pdf","description":"SVHC Statement","material":"Delrin\u00ae 100P NC010","mrl_id":11804,"doc_id":775}],"name":"Regulatory","type":"Doc","icon":"regulatory100","pos":7},{"name":"Product information","namev":"Value","groups":[{"content":[{"groupName":"Product information","name":"Resin Identification","id":915,"key":"Spt-915","state":0,"options":["text"],"unit":"","standard":"ISO 1043","value":"POM","tabbed":0},{"groupName":"Product information","name":"Part Marking Code","id":895,"key":"Spt-895","state":0,"options":["text"],"unit":"","standard":"ISO 11469","value":">POM<","tabbed":0}],"emptyUnit":true,"emptyStd":false}],"pos":8,"type":"Spt"},{"name":"Rheological properties","namev":"Value","groups":[{"content":[{"groupName":"Rheological properties","name":"Melt volume-flow rate","id":1,"key":"Spt-1","state":0,"options":[],"unit":"cm\u00b3\/10min","standard":"ISO 1133","value":"2.1","tabbed":0},{"groupName":"Rheological properties","name":"Melt mass-flow rate","id":560,"key":"Spt-560","state":0,"options":[],"unit":"g\/10min","standard":"ISO 1133","value":"2.5","tabbed":0},{"groupName":"Rheological properties","name":"Temperature","id":2,"key":"Spt-2","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 1133","value":"190","tabbed":0},{"groupName":"Rheological properties","name":"Load","id":3,"key":"Spt-3","state":0,"options":[],"unit":"kg","standard":"ISO 1133","value":"2.16","tabbed":0},{"groupName":"Rheological properties","name":"Melt mass-flow rate, Temperature","id":820,"key":"Spt-820","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 1133","value":"190","tabbed":0},{"groupName":"Rheological properties","name":"Melt mass-flow rate, Load","id":819,"key":"Spt-819","state":0,"options":[],"unit":"kg","standard":"ISO 1133","value":"2.16","tabbed":0},{"groupName":"Rheological properties","name":"Moulding shrinkage, parallel","id":4,"key":"Spt-4","state":0,"options":[],"unit":"%","standard":"ISO 294-4","value":"2.2","tabbed":0},{"groupName":"Rheological properties","name":"Moulding shrinkage, normal","id":5,"key":"Spt-5","state":0,"options":[],"unit":"%","standard":"ISO 294-4","value":"1.9","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":9,"type":"Spt"},{"name":"Mechanical properties","namev":"Value","groups":[{"content":[{"groupName":"Mechanical properties","name":"Tensile Modulus","id":6,"key":"Spt-6","state":0,"options":[],"unit":"MPa","standard":"ISO 527-1\/-2","value":"2900","tabbed":0},{"groupName":"Mechanical properties","name":"Yield stress","id":7,"key":"Spt-7","state":0,"options":[],"unit":"MPa","standard":"ISO 527-1\/-2","value":"70","tabbed":0},{"groupName":"Mechanical properties","name":"Yield strain","id":8,"key":"Spt-8","state":0,"options":[],"unit":"%","standard":"ISO 527-1\/-2","value":"26","tabbed":0},{"groupName":"Mechanical properties","name":"Nominal strain at break","id":9,"key":"Spt-9","state":0,"options":[],"unit":"%","standard":"ISO 527-1\/-2","value":"45","tabbed":0},{"groupName":"Mechanical properties","name":"Flexural Modulus","id":754,"key":"Spt-754","state":0,"options":[],"unit":"MPa","standard":"ISO 178","value":"2800","tabbed":0},{"groupName":"Mechanical properties","name":"Flexural Stress at 3.5%","id":758,"key":"Spt-758","state":0,"options":[],"unit":"MPa","standard":"ISO 178","value":"75","tabbed":0},{"groupName":"Mechanical properties","name":"Tensile creep modulus, 1h","id":13,"key":"Spt-13","state":0,"options":[],"unit":"MPa","standard":"ISO 899-1","value":"2700","tabbed":0},{"groupName":"Mechanical properties","name":"Tensile creep modulus, 1000h","id":14,"key":"Spt-14","state":0,"options":[],"unit":"MPa","standard":"ISO 899-1","value":"1500","tabbed":0},{"groupName":"Mechanical properties","name":"Charpy impact strength, 23\u00b0C","id":15,"key":"Spt-15","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 179\/1eU","value":"N","tabbed":0},{"groupName":"Mechanical properties","name":"Charpy impact strength, -30\u00b0C","id":16,"key":"Spt-16","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 179\/1eU","value":"400","tabbed":0},{"groupName":"Mechanical properties","name":"Charpy notched impact strength, 23\u00b0C","id":17,"key":"Spt-17","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 179\/1eA","value":"14","tabbed":0},{"groupName":"Mechanical properties","name":"Charpy notched impact strength, -30\u00b0C","id":18,"key":"Spt-18","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 179\/1eA","value":"13","tabbed":0},{"groupName":"Mechanical properties","name":"Izod notched impact strength, 23\u00b0C","id":777,"key":"Spt-777","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 180\/1A","value":"14","tabbed":0},{"groupName":"Mechanical properties","name":"Izod notched impact strength, -40\u00b0C","id":779,"key":"Spt-779","state":0,"options":[],"unit":"kJ\/m\u00b2","standard":"ISO 180\/1A","value":"12","tabbed":0},{"groupName":"Mechanical properties","name":"Hardness, Rockwell, M-scale","id":715,"key":"Spt-715","state":0,"options":[],"unit":"","standard":"ISO 2039-2","value":"88","tabbed":0},{"groupName":"Mechanical properties","name":"Hardness, Rockwell, R-scale","id":716,"key":"Spt-716","state":0,"options":[],"unit":"","standard":"ISO 2039-2","value":"119","tabbed":0},{"groupName":"Mechanical properties","name":"Ball indentation hardness, H 358\/30","id":713,"key":"Spt-713","state":0,"options":[],"unit":"MPa","standard":"ISO 2039-1","value":"173","tabbed":0},{"groupName":"Mechanical properties","name":"Poisson's ratio","id":1038,"key":"Spt-1038","state":0,"options":[],"unit":"","standard":"","value":"0.37","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":10,"type":"Spt"},{"name":"Thermal properties","namev":"Value","groups":[{"content":[{"groupName":"Thermal properties","name":"Melting temperature, 10\u00b0C\/min","id":24,"key":"Spt-24","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 11357-1\/-3","value":"178","tabbed":0},{"groupName":"Thermal properties","name":"Temp. of deflection under load, 1.8 MPa","id":26,"key":"Spt-26","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 75-1\/-2","value":"95","tabbed":0},{"groupName":"Thermal properties","name":"Temp. of deflection under load,  1.8 MPa, annealed","id":688,"key":"Spt-688","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 75-1\/-2","value":"110","tabbed":0},{"groupName":"Thermal properties","name":"Temp. of deflection under load, 0.45 MPa","id":27,"key":"Spt-27","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 75-1\/-2","value":"155","tabbed":0},{"groupName":"Thermal properties","name":"Vicat softening temperature, 50\u00b0C\/h, 50N","id":29,"key":"Spt-29","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 306","value":"160","tabbed":0},{"groupName":"Thermal properties","name":"Vicat softening temperature, 50\u00b0C\/h 10N","id":1281,"key":"Spt-1281","state":0,"options":[],"unit":"\u00b0C","standard":"ISO 306","value":"175","tabbed":0},{"groupName":"Thermal properties","name":"Coeff. of linear therm. expansion, parallel","id":477,"key":"Spt-477","state":0,"options":[],"unit":"E-6\/K","standard":"ISO 11359-1\/-2","value":"110","tabbed":0},{"groupName":"Thermal properties","name":"Coeff. of linear therm. expansion, normal","id":478,"key":"Spt-478","state":0,"options":[],"unit":"E-6\/K","standard":"ISO 11359-1\/-2","value":"110","tabbed":0},{"groupName":"Thermal properties","name":"Coeff. of linear therm. expansion,   normal, -40-23\u00b0C","id":829,"key":"Spt-829","state":0,"options":[],"unit":"E-6\/K","standard":"ISO 11359-1\/-2","value":"100","tabbed":0},{"groupName":"Thermal properties","name":"Coeff. of linear therm. expansion,  parallel, -40-23\u00b0C","id":832,"key":"Spt-832","state":0,"options":[],"unit":"E-6\/K","standard":"ISO 11359-1\/-2","value":"100","tabbed":0},{"groupName":"Thermal properties","name":"Thermal conductivity of melt","id":176,"key":"Spt-176","state":0,"options":[],"unit":"W\/(m K)","standard":"ISO 22007-2","value":"0.22","tabbed":0},{"groupName":"Thermal properties","name":"Spec. heat capacity of melt","id":177,"key":"Spt-177","state":0,"options":[],"unit":"J\/(kg K)","standard":"","value":"3000","tabbed":0},{"groupName":"Thermal properties","name":"RTI, electrical, 0.75mm","id":950,"key":"Spt-950","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"50","tabbed":0},{"groupName":"Thermal properties","name":"RTI, electrical, 1.5mm","id":684,"key":"Spt-684","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"110","tabbed":0},{"groupName":"Thermal properties","name":"RTI, electrical, 3mm","id":951,"key":"Spt-951","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"110","tabbed":0},{"groupName":"Thermal properties","name":"RTI, impact, 0.75mm","id":953,"key":"Spt-953","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"50","tabbed":0},{"groupName":"Thermal properties","name":"RTI, impact, 1.5mm","id":685,"key":"Spt-685","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"85","tabbed":0},{"groupName":"Thermal properties","name":"RTI, impact, 3mm","id":954,"key":"Spt-954","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"90","tabbed":0},{"groupName":"Thermal properties","name":"RTI, strength, 0.75mm","id":956,"key":"Spt-956","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"50","tabbed":0},{"groupName":"Thermal properties","name":"RTI, strength, 1.5mm","id":686,"key":"Spt-686","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"90","tabbed":0},{"groupName":"Thermal properties","name":"RTI, strength, 3mm","id":957,"key":"Spt-957","state":0,"options":[],"unit":"\u00b0C","standard":"UL 746B","value":"95","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":11,"type":"Spt"},{"name":"Flammability","namev":"Value","groups":[{"content":[{"groupName":"Flammability","name":"Burning Behav. at 1.5mm nom. thickn.","id":32,"key":"Spt-32","state":0,"options":[],"unit":"class","standard":"IEC 60695-11-10","value":"HB","tabbed":0},{"groupName":"Flammability","name":"Thickness tested","id":33,"key":"Spt-33","state":0,"options":[],"unit":"mm","standard":"IEC 60695-11-10","value":"1.5","tabbed":1},{"groupName":"Flammability","name":"UL recognition","id":34,"key":"Spt-34","state":0,"options":[],"unit":"","standard":"UL 94","value":"yes","tabbed":1},{"groupName":"Flammability","name":"Burning Behav. at thickness h","id":35,"key":"Spt-35","state":0,"options":[],"unit":"class","standard":"IEC 60695-11-10","value":"HB","tabbed":0},{"groupName":"Flammability","name":"Thickness tested","id":36,"key":"Spt-36","state":0,"options":[],"unit":"mm","standard":"IEC 60695-11-10","value":"0.8","tabbed":1},{"groupName":"Flammability","name":"UL recognition","id":37,"key":"Spt-37","state":0,"options":[],"unit":"","standard":"UL 94","value":"yes","tabbed":1},{"groupName":"Flammability","name":"Glow Wire Flammability Index, 1mm","id":692,"key":"Spt-692","state":0,"options":[],"unit":"\u00b0C","standard":"IEC 60695-2-12","value":"550","tabbed":0},{"groupName":"Flammability","name":"Glow Wire Flammability Index, 2mm","id":693,"key":"Spt-693","state":0,"options":[],"unit":"\u00b0C","standard":"IEC 60695-2-12","value":"550","tabbed":0},{"groupName":"Flammability","name":"Glow Wire Flammability Index, 3mm","id":694,"key":"Spt-694","state":0,"options":[],"unit":"\u00b0C","standard":"IEC 60695-2-12","value":"550","tabbed":0},{"groupName":"Flammability","name":"FMVSS Class","id":1069,"key":"Spt-1069","state":0,"options":[],"unit":"","standard":"ISO 3795 (FMVSS 302)","value":"B","tabbed":0},{"groupName":"Flammability","name":"Burning rate, Thickness 1 mm","id":502,"key":"Spt-502","state":0,"options":[],"unit":"mm\/min","standard":"ISO 3795 (FMVSS 302)","value":"26","tabbed":0,"annotations":{"c0":"2 mm"}}],"emptyUnit":false,"emptyStd":false}],"pos":12,"type":"Spt"},{"name":"Electrical properties","namev":"Value","groups":[{"content":[{"groupName":"Electrical properties","name":"Relative permittivity, 100Hz","id":42,"key":"Spt-42","state":0,"options":[],"unit":"","standard":"IEC 62631-2-1","value":"3.9","tabbed":0},{"groupName":"Electrical properties","name":"Relative permittivity, 1MHz","id":43,"key":"Spt-43","state":0,"options":[],"unit":"","standard":"IEC 62631-2-1","value":"3.9","tabbed":0},{"groupName":"Electrical properties","name":"Dissipation factor, 100Hz","id":44,"key":"Spt-44","state":0,"options":[],"unit":"E-4","standard":"IEC 62631-2-1","value":"35","tabbed":0},{"groupName":"Electrical properties","name":"Dissipation factor, 1MHz","id":45,"key":"Spt-45","state":0,"options":[],"unit":"E-4","standard":"IEC 62631-2-1","value":"55","tabbed":0},{"groupName":"Electrical properties","name":"Volume resistivity","id":46,"key":"Spt-46","state":0,"options":[],"unit":"Ohm.m","standard":"IEC 62631-3-1","value":"1E12","tabbed":0},{"groupName":"Electrical properties","name":"Surface resistivity","id":47,"key":"Spt-47","state":0,"options":[],"unit":"Ohm","standard":"IEC 62631-3-2","value":"2E13","tabbed":0},{"groupName":"Electrical properties","name":"Electric strength","id":48,"key":"Spt-48","state":0,"options":[],"unit":"kV\/mm","standard":"IEC 60243-1","value":"41","tabbed":0},{"groupName":"Electrical properties","name":"Comparative tracking index","id":49,"key":"Spt-49","state":0,"options":[],"unit":"","standard":"IEC 60112","value":"600","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":13,"type":"Spt"},{"name":"Other properties","namev":"Value","groups":[{"content":[{"groupName":"Other properties","name":"Humidity absorption, 2mm","id":51,"key":"Spt-51","state":0,"options":[],"unit":"%","standard":"Sim. to ISO 62","value":"0.3","tabbed":0},{"groupName":"Other properties","name":"Water absorption, 2mm","id":50,"key":"Spt-50","state":0,"options":[],"unit":"%","standard":"Sim. to ISO 62","value":"1.4","tabbed":0},{"groupName":"Other properties","name":"Water absorption, Immersion 24h","id":817,"key":"Spt-817","state":0,"options":[],"unit":"%","standard":"Sim. to ISO 62","value":"0.4","tabbed":0},{"groupName":"Other properties","name":"Density","id":52,"key":"Spt-52","state":0,"options":[],"unit":"kg\/m\u00b3","standard":"ISO 1183","value":"1420","tabbed":0},{"groupName":"Other properties","name":"Density of melt","id":175,"key":"Spt-175","state":0,"options":[],"unit":"kg\/m\u00b3","standard":"","value":"1190","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":14,"type":"Spt"},{"name":"VDA Properties","namev":"Value","groups":[{"content":[{"groupName":"VDA Properties","name":"Emissions","id":810,"key":"Spt-810","state":0,"options":[],"unit":"mg\/kg","standard":"VDA 275","value":"<8","tabbed":0},{"groupName":"VDA Properties","name":"Emission of organic compounds","id":518,"key":"Spt-518","state":0,"options":[],"unit":"\u00b5gC\/g","standard":"VDA 277","value":"4.7","tabbed":0},{"groupName":"VDA Properties","name":"Fogging, F-value (refraction)","id":808,"key":"Spt-808","state":0,"options":[],"unit":"%","standard":"ISO 6452","value":"91","tabbed":0}],"emptyUnit":false,"emptyStd":false}],"pos":15,"type":"Spt"},{"name":"Injection","namev":"Value","groups":[{"content":[{"groupName":"Injection","name":"Drying Recommended","id":939,"key":"Spt-939","state":0,"options":[],"unit":"","standard":"","value":"yes","tabbed":0},{"groupName":"Injection","name":"Drying Temperature","id":940,"key":"Spt-940","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"80","tabbed":0},{"groupName":"Injection","name":"Drying Time, Dehumidified Dryer","id":941,"key":"Spt-941","state":0,"options":[],"unit":"h","standard":"","value":"2 - 4","tabbed":0},{"groupName":"Injection","name":"Processing Moisture Content","id":944,"key":"Spt-944","state":0,"options":[],"unit":"%","standard":"","value":"\u22640.2","tabbed":0},{"groupName":"Injection","name":"Melt Temperature Optimum","id":942,"key":"Spt-942","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"215","tabbed":0},{"groupName":"Injection","name":"Min. melt temperature","id":109,"key":"Spt-109","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"210","tabbed":0},{"groupName":"Injection","name":"Max. melt temperature","id":110,"key":"Spt-110","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"220","tabbed":0},{"groupName":"Injection","name":"Max. screw tangential speed","id":1035,"key":"Spt-1035","state":0,"options":[],"unit":"m\/s","standard":"","value":"0.2","tabbed":0},{"groupName":"Injection","name":"Mold Temperature Optimum","id":943,"key":"Spt-943","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"90","tabbed":0},{"groupName":"Injection","name":"Min. mould temperature","id":103,"key":"Spt-103","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"80","tabbed":0},{"groupName":"Injection","name":"Max. mould temperature","id":105,"key":"Spt-105","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"100","tabbed":0},{"groupName":"Injection","name":"Hold pressure range","id":1029,"key":"Spt-1029","state":0,"options":[],"unit":"MPa","standard":"","value":"90 - 110","tabbed":0},{"groupName":"Injection","name":"Hold pressure time","id":1030,"key":"Spt-1030","state":0,"options":[],"unit":"s\/mm","standard":"","value":"8","tabbed":0},{"groupName":"Injection","name":"Annealing time, optional","id":1058,"key":"Spt-1058","state":0,"options":[],"unit":"min\/mm","standard":"","value":"30","tabbed":0},{"groupName":"Injection","name":"Annealing temperature","id":1061,"key":"Spt-1061","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"160","tabbed":0}],"emptyUnit":false,"emptyStd":true}],"pos":16,"type":"Spt"},{"name":"Extrusion","namev":"Value","groups":[{"content":[{"groupName":"Extrusion","name":"Drying Temperature","id":965,"key":"Spt-965","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"80","tabbed":0},{"groupName":"Extrusion","name":"Drying Time, Dehumidified Dryer","id":966,"key":"Spt-966","state":0,"options":[],"unit":"h","standard":"","value":"2 - 4","tabbed":0},{"groupName":"Extrusion","name":"Processing Moisture Content","id":964,"key":"Spt-964","state":0,"options":[],"unit":"%","standard":"","value":"\u22640.2","tabbed":0},{"groupName":"Extrusion","name":"Melt Temperature Optimum","id":962,"key":"Spt-962","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"200","tabbed":0},{"groupName":"Extrusion","name":"Melt Temperature Range","id":963,"key":"Spt-963","state":0,"options":[],"unit":"\u00b0C","standard":"","value":"195 - 205","tabbed":0}],"emptyUnit":false,"emptyStd":true}],"pos":17,"type":"Spt"},{"cattype":"processing_txt","name":"Additional information","content":[{"name":"Injection molding","content":"<p><span>Drying is recommended, but not necessary for newly opened packaging stored in a dry location.<\/span>\n<\/p>\n\n<div>Follow the drying guidelines above in the following cases:\n<p class=\"MsoListParagraph\">\u00b7\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0If moisture is above the Processing Moisture Content recommendation,<\/p>\n\n<p class=\"MsoListParagraph\">\u00b7\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0When a resin container is damaged,<\/p>\n\n<p class=\"MsoListParagraph\">\u00b7\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0When the material is not properly stored in a dry place at room temperature, or<\/p>\n\n<p class=\"MsoListParagraph\">\u00b7\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0\u00a0When packaging stays open for a significant time.<\/p>\n<\/div>\n\n"}],"protectxt":[],"pos":18,"type":"Text"},{"content":[{"gname":"Acids","content":[{"name":"Acetic Acid (5% by mass), 23\u00b0C","chemid":101,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Citric Acid solution (10% by mass), 23\u00b0C","chemid":102,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Lactic Acid (10% by mass), 23\u00b0C","chemid":103,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Hydrochloric Acid (36% by mass), 23\u00b0C","chemid":104,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Nitric Acid (40% by mass), 23\u00b0C","chemid":105,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Sulfuric Acid (38% by mass), 23\u00b0C","chemid":106,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Sulfuric Acid (5% by mass), 23\u00b0C","chemid":107,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Chromic Acid solution (40% by mass), 23\u00b0C","chemid":108,"textid":null,"text":"","text2":"","ltha":false,"value":0}],"type":"Chem"},{"gname":"Bases","content":[{"name":"Sodium Hydroxide solution (35% by mass), 23\u00b0C","chemid":201,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Sodium Hydroxide solution (1% by mass), 23\u00b0C","chemid":202,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Ammonium Hydroxide solution (10% by mass), 23\u00b0C","chemid":203,"textid":null,"text":"","text2":"","ltha":false,"value":0}],"type":"Chem"},{"gname":"Alcohols","content":[{"name":"Isopropyl alcohol, 23\u00b0C","chemid":301,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Methanol, 23\u00b0C","chemid":302,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Ethanol, 23\u00b0C","chemid":303,"textid":null,"text":"","text2":"","ltha":false,"value":1}],"type":"Chem"},{"gname":"Hydrocarbons","content":[{"name":"n-Hexane, 23\u00b0C","chemid":401,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Toluene, 23\u00b0C","chemid":402,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"iso-Octane, 23\u00b0C","chemid":403,"textid":null,"text":"","text2":"","ltha":false,"value":1}],"type":"Chem"},{"gname":"Ketones","content":[{"name":"Acetone, 23\u00b0C","chemid":501,"textid":null,"text":"","text2":"","ltha":false,"value":1}],"type":"Chem"},{"gname":"Ethers","content":[{"name":"Diethyl ether, 23\u00b0C","chemid":601,"textid":null,"text":"","text2":"","ltha":false,"value":1}],"type":"Chem"},{"gname":"Mineral oils","content":[{"name":"SAE 10W40 multigrade motor oil, 23\u00b0C","chemid":701,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"SAE 10W40 multigrade motor oil, 130\u00b0C","chemid":702,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"SAE 80\/90 hypoid-gear oil, 130\u00b0C","chemid":703,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Insulating Oil, 23\u00b0C","chemid":704,"textid":null,"text":"","text2":"","ltha":false,"value":1}],"type":"Chem"},{"gname":"Standard Fuels","content":[{"name":"ISO 1817 Liquid 1 - E5, 60\u00b0C","chemid":801,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"ISO 1817 Liquid 2 - M15E4, 60\u00b0C","chemid":802,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"ISO 1817 Liquid 3 - M3E7, 60\u00b0C","chemid":803,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"ISO 1817 Liquid 4 - M15, 60\u00b0C","chemid":804,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Standard fuel without alcohol (pref. ISO 1817 Liquid C), 23\u00b0C","chemid":805,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Standard fuel with alcohol (pref. ISO 1817 Liquid 4), 23\u00b0C","chemid":806,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Diesel fuel (pref. ISO 1817 Liquid F), 23\u00b0C","chemid":807,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Diesel fuel (pref. ISO 1817 Liquid F), 90\u00b0C","chemid":808,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Diesel fuel (pref. ISO 1817 Liquid F), >90\u00b0C","chemid":809,"textid":null,"text":"","text2":"","ltha":false,"value":0}],"type":"Chem"},{"gname":"Salt solutions","content":[{"name":"Sodium Chloride solution (10% by mass), 23\u00b0C","chemid":901,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Sodium Hypochlorite solution (10% by mass), 23\u00b0C","chemid":902,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Sodium Carbonate solution (20% by mass), 23\u00b0C","chemid":903,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Sodium Carbonate solution (2% by mass), 23\u00b0C","chemid":904,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Zinc Chloride solution (50% by mass), 23\u00b0C","chemid":905,"textid":null,"text":"","text2":"","ltha":false,"value":0}],"type":"Chem"},{"gname":"Other","content":[{"name":"Ethyl Acetate, 23\u00b0C","chemid":1001,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Hydrogen peroxide, 23\u00b0C","chemid":1002,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"DOT No. 4 Brake fluid, 130\u00b0C","chemid":1003,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Ethylene Glycol (50% by mass) in water, 108\u00b0C","chemid":1004,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"1% nonylphenoxy-polyethyleneoxy ethanol in water, 23\u00b0C","chemid":1005,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"50% Oleic acid + 50% Olive Oil, 23\u00b0C","chemid":1006,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Water, 23\u00b0C","chemid":1007,"textid":null,"text":"","text2":"","ltha":false,"value":1},{"name":"Water, 90\u00b0C","chemid":1008,"textid":null,"text":"","text2":"","ltha":false,"value":0},{"name":"Phenol solution (5% by mass), 23\u00b0C","chemid":1009,"textid":null,"text":"","text2":"","ltha":false,"value":0}],"type":"Chem"}],"name":"Chemical Media Resistance","pos":19,"type":"Chem"},{"content":[{"id":1,"addId":[],"data":{"name":"Viscosity-shear rate ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Shear rate in","unit":"1\/s","log":true},"y":{"name":"Viscosity in","unit":"Pa.s","log":true},"z":{"name":"","unit":"\u00b0C"}},"x":[[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463],[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463],[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463]],"y":[[1770.4399999999991,1728.5294865424478,1687.5563025048875,1647.4473688293679,1608.1350782081063,1569.5570266184038,1531.655769615046,1494.378600506318,1457.6773477460808,1421.5081890602157,1385.8314799945222,1350.6115947256544,1315.8167771195037,1281.422778590653,1247.4380876708001,1213.8849261580215,1180.7839583250577,1148.1542227491307,1116.0131636105925,1084.3766650994098,1053.2590886362843,1022.6733126203382,992.63077442157794,963.14151434356927,934.2142212898874,905.85627987685132,878.07381874463795,850.87175982904159,824.25386836686835,798.22263801842189,772.77724994794323,747.91455302705231,723.63091245739088,699.92227219113863,676.78417428702721,654.21177822764275,632.19988016316108,610.74293204807543,589.83506063888524,569.47008632218603,549.6415417440752,530.34264036771424,511.564332367887,493.29501321622973,475.52333683504986,458.23839012975395,441.42966406050084,425.08702609335757,409.20069398142948,393.76121083037248,378.75942140622425,364.18644964672745,350.0336773401836,336.29273228960011,322.95841209292161,310.03229198582687,297.51558724169291,285.40805945594587,273.70813780940563,262.41303739114414,251.5188739907183,241.02077486328636,230.91298505940452,221.18896899382543,211.8415070040912,202.86278671996973,194.24448912875388,185.97786927914765,178.05383161803636,170.46300000000394],[1631.6899999999998,1594.6998115625354,1558.4906543359141,1522.9912162956109,1488.1355790735588,1453.8629706838633,1420.1175442070169,1386.8481792492132,1354.008303204474,1321.5557295357444,1289.4525104607192,1257.6648015827793,1226.1627361502151,1194.9243117156288,1163.9621905974282,1133.3036454348032,1102.9743565369663,1072.9983224648083,1043.3978772027549,1014.1937118355685,985.40490039685494,957.04892955619084,929.14173181374349,901.69772187485967,874.72983588226271,848.24957319006137,822.26704037153911,796.79099716168594,771.82890404531645,747.38679583496332,723.46711420128611,700.0697457084766,677.19398105368509,654.83858037051675,633.00179313327681,611.68137827396015,590.87462446171094,570.57837049590717,550.78902576548148,531.50259072867539,512.71467736905311,494.42047659876033,476.61269412045067,459.28124944114256,442.41627132562178,426.00828436062437,410.04817903785886,394.52718324197025,379.43683510029808,364.76895715539393,350.51563182497955,336.66917811731628,323.22212957283938,310.16722216947403,297.5004591315095,285.22486789086526,273.34299086230493,261.85574288603812,250.76254573346449,240.0614598410335,229.74931248638035,219.82182174124517,210.2737156495663,201.0988461859034,192.29029764845671,183.84048923215437,175.74127161034903,167.98401742864752,160.55970568133841,153.4590000000037],[1458.3000000000002,1427.531621399419,1397.3539234739771,1367.6996653239926,1338.5066193998261,1309.7173682285213,1281.279127265519,1253.1435905319424,1225.2667958877723,1197.6090069570623,1170.1346088679777,1142.812015102237,1115.6135828696711,1088.5196723830702,1061.5464345942648,1034.7252569869909,1008.0860407480793,981.65708467627837,955.46508034878093,929.53511322407564,903.89066934976734,878.55364733491854,853.5443752399251,828.88163203291276,804.58267325993438,780.66326057671176,757.13769479217945,734.01885207845885,711.31822300798297,689.04577019843316,667.20764584347899,645.80726955339924,624.84737696280627,604.330084562396,584.25690732688508,564.62877693583903,545.44606052297388,526.70857989031799,508.41563112462654,490.56600455457999,473.15800498862006,456.18941685931185,439.65534938803745,423.54792542244957,407.85941119579047,392.58241241245088,377.70984414650684,363.23490207485213,349.15103501601243,335.45191874989922,322.13143109745482,309.18362824231673,296.60272227935684,284.3830690842023,272.52235053625895,261.02545602140339,249.89666375589761,239.13845613538876,228.75166423330535,218.73561016759129,209.08824630431232,199.80629041637175,190.88535605813388,182.32007755110484,174.10422910111052,166.23083768309522,158.69228943537337,151.48042940078639,144.58665453776942,138.00200000000356]],"xo":[[100,200,500,1000,2000,5000],[100,200,500,1000,2000,5000],[100,200,500,1000,2000,5000]],"yo":[[1770.4400000000001,1308.02,814.10599999999999,537.75199999999995,338.48399999999998,170.46299999999999],[1631.6900000000001,1219.0899999999999,762.30399999999997,501.44499999999999,312.24900000000002,153.459],[1458.3,1109.49,702.64400000000001,462.70699999999999,286.33199999999999,138.00200000000001]],"z":[{"value":200,"unit":"\u00b0C","name":"","comment":null,"realZ":200},{"value":215,"unit":"\u00b0C","name":"","comment":null,"realZ":215},{"value":230,"unit":"\u00b0C","name":"","comment":null,"realZ":230}],"zo":[{"value":200,"unit":"\u00b0C","name":"","comment":null,"realZ":200},{"value":215,"unit":"\u00b0C","name":"","comment":null,"realZ":215},{"value":230,"unit":"\u00b0C","name":"","comment":null,"realZ":230}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"viscosity-shear-rate-delrin\u00ae-100p-nc010.png","svgname":"viscosity-shear-rate-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","",""],"xmarker":[],"option":1},"moist":0,"name":"Viscosity-shear rate","shortname":"&#951;-&#947;<sup>.<\/sup>"},{"id":29,"addId":[],"data":{"name":"Shearstress-shear rate ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Shear rate in","unit":"1\/s","log":true},"y":{"name":"Shearstress in","unit":"Pa","log":true},"z":{"name":"","unit":"\u00b0C"}},"x":[[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463],[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463],[100,105.8334012687634,112.00708824115091,118.54091114771515,125.45587816260966,132.77422295108562,140.51947615730498,148.71654106232489,157.39177365551561,166.57306737686568,176.28994280264587,186.57364256279769,197.45723179523404,208.97570446004232,221.16609585542167,234.06760169712632,247.72170414429056,262.17230517684595,277.46586775337835,293.65156520328929,310.78143933360155,328.91056775876905,348.09724099150594,368.4031498640349,389.89358388236781,412.63764115138895,436.70845054570947,462.18340684063986,489.14441955929567,517.67817633595303,547.87642164244573,579.83625177379167,613.66042704151425,649.45770217845291,687.34317601741236,727.43866156797071,769.87307768135224,814.78286356268416,862.31241746341652,912.61456096443192,965.85103034265057,1022.1929966010232,1081.8216158339578,1144.9286116977728,1211.7168918589857,1282.4012004025083,1357.2088082974253,1436.3802441404162,1520.1700675263701,1608.8476875328147,1702.6982289498246,1802.0234490405956,1907.1427077803437,2018.3939946931312,2136.1350155882046,2260.7443426900263,2392.6226318600029,2532.1939108236447,2679.9069425451808,2836.2366681332901,3001.6857339173102,3176.7861076039326,3362.1007887107999,3558.2256187765602,3765.7911971677363,3985.4649086422996,4217.9530691891596,4464.0031970430846,4724.4064161770348,4999.9999999998463]],"y":[[177043.99999999991,182936.15413224432,189018.26642740701,195289.91028459184,201749.99597446754,208396.71161705532,215227.46304452838,222238.81292613965,229426.41958737359,236784.97601218452,244308.14957513727,251988.52310873615,259817.5379694335,267786.22941152274,275891.0156311132,284131.14015996386,292505.82420924393,301014.25231510075,309655.57711471221,318428.92427545297,327333.39756791946,336368.08407352632,345532.0595173678,354824.39371711551,364244.15613880556,373790.42155051796,383462.27576514793,393258.82146369922,403179.18409081071,413222.43223803589,423386.41331556003,433667.93472665671,444063.60279441765,454569.84380508371,465182.90426878777,475898.85145482171,486713.57420627115,497622.78403838276,508622.01652451564,519706.63297300925,530871.82239776617,542112.55279359804,553421.43437616364,564787.73094177467,576199.90122244449,587645.79646568431,599112.66208727541,610587.14157370199,622055.28275753453,633502.54658467555,644913.81848694407,656273.42246690497,667565.13799411873,678772.23666245118,689883.79752428632,700904.77141070121,711843.52234581113,722709.49691692577,733513.21575871122,744266.26568854006,754981.29293742392,765671.99792124867,776353.13199732278,787040.49665179697,797750.94556480797,808502.39000272937,819313.80799091246,830205.25772645499,841197.89569910977,852313.99999999476],[163168.99999999997,168772.58865393981,174562.17203809071,180537.03004683371,186695.71372253491,193035.97932938079,199554.72132056713,206247.90468035132,213110.4971925024,220136.40225871903,227318.39296373309,234648.04815712778,242115.69139415026,249711.17087871546,257430.00552534318,265270.69174379396,273231.68912063556,281311.4060441475,289508.20561216737,297820.41170916607,306246.315237756,314784.18048977829,323432.25164214778,332188.75936270144,341051.927511496,350019.97992320603,359091.14725659974,368263.67389743176,377535.82490151888,386905.80192591588,396370.50538246473,405925.72884529579,415567.05336544331,425289.87164299213,435089.39016201871,444960.63168921648,454898.43813870987,464897.47380468738,474952.22896266787,485057.02383933833,495206.01295002631,505393.13571792934,515609.85405980324,525844.11539230216,536083.05821565073,546313.22864591598,556520.5894242333,566690.53171706432,576807.88982734713,586856.95892750181,596821.51591509697,606684.84348018526,616429.7574602149,626038.65522821574,635500.14205733011,644819.52907894354,654005.70741263288,663068.68672154809,672019.57234267984,680870.54311269172,689634.83043094899,698326.69909236324,706961.43041328422,715555.30816461367,724125.60781805823,732690.58960454294,741269.49587903812,749882.55328365683,758550.98020172725,767296.99999999511],[145830.00000000003,151080.60891351194,156513.71301111041,162128.62393535476,167923.87612076267,173897.15330455435,180045.21376184348,186363.81485407607,192847.63756840018,199490.21181703394,206283.84335840755,213219.54329447125,220286.96118942826,227475.18794041598,234779.11623479857,242196.69054597791,249725.80169935862,257364.27301606277,265109.86742295854,272960.2947675102,280913.21931602323,288966.26741372584,297117.0352851362,305363.09695324558,313702.01225628325,322131.33494113054,330648.62081288238,339251.43592057482,347937.36475970509,356703.92304241663,365547.2604309803,374462.36336827796,383443.99335864885,392486.71399688814,401584.89499154134,410732.71665240801,419924.17484163254,429153.08638646075,438413.09495046613,447697.67735873023,457000.15037114581,466313.62140943075,475628.62858986831,484932.0640553892,494210.00680997851,503447.95530822466,512630.84371083917,521743.06149957224,530768.47656466858,539690.4618637173,548491.92573456618,557155.34592694079,565662.80739761598,573996.0622717255,582143.42022760271,590110.61549356848,597907.11992405169,605543.56925643072,613031.72588655853,620384.44245971739,627615.62693814491,634740.20978535339,641774.11388595251,648734.22779854049,655638.38291903329,662505.33511357172,669354.75136444869,676207.20196018449,683084.15875257633,690007.99999999627]],"xo":[[100,200,500,1000,2000,5000],[100,200,500,1000,2000,5000],[100,200,500,1000,2000,5000]],"yo":[[177044,261604,407053,537752,676969,852314],[163169,243819,381152,501445,624497,767297],[145830,221899,351322,462707,572663,690008]],"z":[{"value":200,"unit":"\u00b0C","name":"","comment":null,"realZ":200},{"value":215,"unit":"\u00b0C","name":"","comment":null,"realZ":215},{"value":230,"unit":"\u00b0C","name":"","comment":null,"realZ":230}],"zo":[{"value":200,"unit":"\u00b0C","name":"","comment":null,"realZ":200},{"value":215,"unit":"\u00b0C","name":"","comment":null,"realZ":215},{"value":230,"unit":"\u00b0C","name":"","comment":null,"realZ":230}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"shearstress-shear-rate-delrin\u00ae-100p-nc010.png","svgname":"shearstress-shear-rate-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","",""],"xmarker":[],"option":1},"moist":0,"name":"Shearstress-shear rate","shortname":"&#964;-&#947;<sup>.<\/sup>"},{"id":3,"addId":[],"data":{"name":"Stress-strain ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"P","axes":{"x":{"name":"Strain in","unit":"%","log":false},"y":{"name":"Stress in","unit":"MPa","log":false},"z":{"name":"","unit":"\u00b0C"}},"x":[[0,0.60289855072463772,1.2057971014492754,1.8086956521739133,2.4115942028985509,3.0144927536231885,3.6173913043478261,4.2202898550724637,4.8231884057971017,5.4260869565217398,6.0289855072463778,6.6318840579710159,7.2347826086956539,7.837681159420292,8.4405797101449291,9.0434782608695663,9.6463768115942035,10.249275362318841,10.852173913043478,11.455072463768115,12.057971014492752,12.660869565217389,13.263768115942026,13.866666666666664,14.469565217391301,15.072463768115938,15.675362318840575,16.278260869565212,16.881159420289851,17.48405797101449,18.086956521739129,18.689855072463768,19.292753623188407,19.895652173913046,20.498550724637685,21.101449275362324,21.704347826086963,22.307246376811602,22.910144927536241,23.513043478260879,24.115942028985518,24.718840579710157,25.321739130434796,25.924637681159435,26.527536231884074,27.130434782608713,27.733333333333352,28.336231884057991,28.93913043478263,29.542028985507269,30.144927536231908,30.747826086956547,31.350724637681186,31.953623188405825,32.55652173913046,33.159420289855099,33.762318840579738,34.365217391304377,34.968115942029016,35.571014492753655,36.173913043478294,36.776811594202933,37.379710144927571,37.98260869565221,38.585507246376849,39.188405797101488,39.791304347826127,40.394202898550766,40.997101449275405,41.600000000000001],[0,0.29999999999999999,0.59999999999999998,0.89999999999999991,1.2,1.5,1.8,2.1000000000000001,2.3999999999999999,2.6999999999999997,2.9999999999999996,3.2999999999999994,3.5999999999999992,3.899999999999999,4.1999999999999993,4.4999999999999991,4.7999999999999989,5.0999999999999988,5.3999999999999986,5.6999999999999984,5.9999999999999982,6.299999999999998,6.5999999999999979,6.8999999999999977,7.1999999999999975,7.4999999999999973,7.7999999999999972,8.0999999999999979,8.3999999999999986,8.6999999999999993,9,9.3000000000000007,9.6000000000000014,9.9000000000000021,10.200000000000003,10.500000000000004,10.800000000000004,11.100000000000005,11.400000000000006,11.700000000000006,12.000000000000007,12.300000000000008,12.600000000000009,12.900000000000009,13.20000000000001,13.500000000000011,13.800000000000011,14.100000000000012,14.400000000000013,14.700000000000014,15.000000000000014,15.300000000000015,15.600000000000016,15.900000000000016,16.200000000000017,16.500000000000018,16.800000000000018,17.100000000000019,17.40000000000002,17.700000000000021,18.000000000000021,18.300000000000022,18.600000000000023,18.900000000000023,19.200000000000024,19.500000000000025,19.800000000000026,20.100000000000026,20.400000000000027,20.699999999999999],[0,0.72463768115942029,1.4492753623188406,2.1739130434782608,2.8985507246376812,3.6231884057971016,4.3478260869565215,5.0724637681159415,5.7971014492753614,6.5217391304347814,7.2463768115942013,7.9710144927536213,8.6956521739130412,9.4202898550724612,10.144927536231881,10.869565217391301,11.594202898550721,12.318840579710141,13.043478260869561,13.768115942028981,14.492753623188401,15.217391304347821,15.942028985507241,16.666666666666661,17.391304347826082,18.115942028985504,18.840579710144926,19.565217391304348,20.289855072463769,21.014492753623191,21.739130434782613,22.463768115942035,23.188405797101456,23.913043478260878,24.6376811594203,25.362318840579722,26.086956521739143,26.811594202898565,27.536231884057987,28.260869565217408,28.98550724637683,29.710144927536252,30.434782608695674,31.159420289855095,31.884057971014517,32.608695652173935,33.333333333333357,34.057971014492779,34.7826086956522,35.507246376811622,36.231884057971044,36.956521739130466,37.681159420289887,38.405797101449309,39.130434782608731,39.855072463768153,40.579710144927574,41.304347826086996,42.028985507246418,42.75362318840584,43.478260869565261,44.202898550724683,44.927536231884105,45.652173913043526,46.376811594202948,47.10144927536237,47.826086956521792,48.550724637681213,49.275362318840635,50],[0,0.85217391304347823,1.7043478260869565,2.5565217391304347,3.4086956521739129,4.2608695652173907,5.1130434782608685,5.9652173913043463,6.817391304347824,7.6695652173913018,8.5217391304347796,9.3739130434782574,10.226086956521735,11.078260869565213,11.930434782608691,12.782608695652169,13.634782608695646,14.486956521739124,15.339130434782602,16.19130434782608,17.043478260869559,17.895652173913039,18.747826086956518,19.599999999999998,20.452173913043477,21.304347826086957,22.156521739130437,23.008695652173916,23.860869565217396,24.713043478260875,25.565217391304355,26.417391304347834,27.269565217391314,28.121739130434793,28.973913043478273,29.826086956521753,30.678260869565232,31.530434782608712,32.382608695652188,33.234782608695667,34.086956521739147,34.939130434782626,35.791304347826106,36.643478260869585,37.495652173913065,38.347826086956545,39.200000000000024,40.052173913043504,40.904347826086983,41.756521739130463,42.608695652173942,43.460869565217422,44.313043478260902,45.165217391304381,46.017391304347861,46.86956521739134,47.72173913043482,48.573913043478299,49.426086956521779,50.278260869565258,51.130434782608738,51.982608695652218,52.834782608695697,53.686956521739177,54.539130434782656,55.391304347826136,56.243478260869615,57.095652173913095,57.947826086956574,58.799999999999997],[0,0.2318840579710145,0.46376811594202899,0.69565217391304346,0.92753623188405798,1.1594202898550725,1.3913043478260869,1.6231884057971013,1.8550724637681157,2.0869565217391304,2.318840579710145,2.5507246376811596,2.7826086956521743,3.0144927536231889,3.2463768115942035,3.4782608695652182,3.7101449275362328,3.9420289855072475,4.1739130434782616,4.4057971014492763,4.6376811594202909,4.8695652173913055,5.1014492753623202,5.3333333333333348,5.5652173913043494,5.7971014492753641,6.0289855072463787,6.2608695652173934,6.492753623188408,6.7246376811594226,6.9565217391304373,7.1884057971014519,7.4202898550724665,7.6521739130434812,7.8840579710144958,8.1159420289855095,8.3478260869565233,8.579710144927537,8.8115942028985508,9.0434782608695645,9.2753623188405783,9.507246376811592,9.7391304347826058,9.9710144927536195,10.202898550724633,10.434782608695647,10.666666666666661,10.898550724637674,11.130434782608688,11.362318840579702,11.594202898550716,11.826086956521729,12.057971014492743,12.289855072463757,12.521739130434771,12.753623188405784,12.985507246376798,13.217391304347812,13.449275362318826,13.681159420289839,13.913043478260853,14.144927536231867,14.376811594202881,14.608695652173894,14.840579710144908,15.072463768115922,15.304347826086936,15.536231884057949,15.768115942028963,15.999999999999977],[0,1.4260869565217391,2.8521739130434782,4.2782608695652176,5.7043478260869565,7.1304347826086953,8.5565217391304351,9.9826086956521749,11.408695652173915,12.834782608695654,14.260869565217394,15.686956521739134,17.113043478260874,18.539130434782614,19.965217391304353,21.391304347826093,22.817391304347833,24.243478260869573,25.669565217391312,27.095652173913052,28.521739130434792,29.947826086956532,31.373913043478272,32.800000000000011,34.226086956521748,35.652173913043484,37.07826086956522,38.504347826086956,39.930434782608693,41.356521739130429,42.782608695652165,44.208695652173901,45.634782608695637,47.060869565217374,48.48695652173911,49.913043478260846,51.339130434782582,52.765217391304319,54.191304347826055,55.617391304347791,57.043478260869527,58.469565217391263,59.895652173913,61.321739130434736,62.747826086956472,64.173913043478208,65.599999999999952,67.026086956521695,68.452173913043438,69.878260869565182,71.304347826086925,72.730434782608668,74.156521739130412,75.582608695652155,77.008695652173898,78.434782608695642,79.860869565217385,81.286956521739128,82.713043478260872,84.139130434782615,85.565217391304358,86.991304347826102,88.417391304347845,89.843478260869588,91.269565217391332,92.695652173913075,94.121739130434818,95.547826086956562,96.973913043478305,98.400000000000006],[0,0.14347826086956522,0.28695652173913044,0.43043478260869567,0.57391304347826089,0.71739130434782616,0.86086956521739144,1.0043478260869567,1.147826086956522,1.2913043478260873,1.4347826086956526,1.5782608695652178,1.7217391304347831,1.8652173913043484,2.0086956521739134,2.1521739130434785,2.2956521739130435,2.4391304347826086,2.5826086956521737,2.7260869565217387,2.8695652173913038,3.0130434782608688,3.1565217391304339,3.2999999999999989,3.443478260869564,3.586956521739129,3.7304347826086941,3.8739130434782592,4.0173913043478242,4.1608695652173893,4.3043478260869543,4.4478260869565194,4.5913043478260844,4.7347826086956495,4.8782608695652145,5.0217391304347796,5.1652173913043447,5.3086956521739097,5.4521739130434748,5.5956521739130398,5.7391304347826049,5.8826086956521699,6.026086956521735,6.1695652173913,6.3130434782608651,6.4565217391304301,6.5999999999999952,6.7434782608695603,6.8869565217391253,7.0304347826086904,7.1739130434782554,7.3173913043478205,7.4608695652173855,7.6043478260869506,7.7478260869565156,7.8913043478260807,8.0347826086956466,8.1782608695652126,8.3217391304347785,8.4652173913043445,8.6086956521739104,8.7521739130434764,8.8956521739130423,9.0391304347826082,9.1826086956521742,9.3260869565217401,9.4695652173913061,9.613043478260872,9.756521739130438,9.9000000000000004],[0,0.72463768115942029,1.4492753623188406,2.1739130434782608,2.8985507246376812,3.6231884057971016,4.3478260869565215,5.0724637681159415,5.7971014492753614,6.5217391304347814,7.2463768115942013,7.9710144927536213,8.6956521739130412,9.4202898550724612,10.144927536231881,10.869565217391301,11.594202898550721,12.318840579710141,13.043478260869561,13.768115942028981,14.492753623188401,15.217391304347821,15.942028985507241,16.666666666666661,17.391304347826082,18.115942028985504,18.840579710144926,19.565217391304348,20.289855072463769,21.014492753623191,21.739130434782613,22.463768115942035,23.188405797101456,23.913043478260878,24.6376811594203,25.362318840579722,26.086956521739143,26.811594202898565,27.536231884057987,28.260869565217408,28.98550724637683,29.710144927536252,30.434782608695674,31.159420289855095,31.884057971014517,32.608695652173935,33.333333333333357,34.057971014492779,34.7826086956522,35.507246376811622,36.231884057971044,36.956521739130466,37.681159420289887,38.405797101449309,39.130434782608731,39.855072463768153,40.579710144927574,41.304347826086996,42.028985507246418,42.75362318840584,43.478260869565261,44.202898550724683,44.927536231884105,45.652173913043526,46.376811594202948,47.10144927536237,47.826086956521792,48.550724637681213,49.275362318840635,50],[0,0.14492753623188406,0.28985507246376813,0.43478260869565222,0.57971014492753625,0.72463768115942029,0.86956521739130432,1.0144927536231885,1.1594202898550725,1.3043478260869565,1.4492753623188406,1.5942028985507246,1.7391304347826086,1.8840579710144927,2.0289855072463769,2.1739130434782612,2.3188405797101455,2.4637681159420297,2.608695652173914,2.7536231884057982,2.8985507246376825,3.0434782608695667,3.188405797101451,3.3333333333333353,3.4782608695652195,3.6231884057971038,3.768115942028988,3.9130434782608723,4.0579710144927565,4.2028985507246404,4.3478260869565242,4.492753623188408,4.6376811594202918,4.7826086956521756,4.9275362318840594,5.0724637681159432,5.2173913043478271,5.3623188405797109,5.5072463768115947,5.6521739130434785,5.7971014492753623,5.9420289855072461,6.0869565217391299,6.2318840579710137,6.3768115942028976,6.5217391304347814,6.6666666666666652,6.811594202898549,6.9565217391304328,7.1014492753623166,7.2463768115942004,7.3913043478260843,7.5362318840579681,7.6811594202898519,7.8260869565217357,7.9710144927536195,8.1159420289855042,8.2608695652173889,8.4057971014492736,8.5507246376811583,8.695652173913043,8.8405797101449277,8.9855072463768124,9.1304347826086971,9.2753623188405818,9.4202898550724665,9.5652173913043512,9.7101449275362359,9.8550724637681206,10],[0,0.72463768115942029,1.4492753623188406,2.1739130434782608,2.8985507246376812,3.6231884057971016,4.3478260869565215,5.0724637681159415,5.7971014492753614,6.5217391304347814,7.2463768115942013,7.9710144927536213,8.6956521739130412,9.4202898550724612,10.144927536231881,10.869565217391301,11.594202898550721,12.318840579710141,13.043478260869561,13.768115942028981,14.492753623188401,15.217391304347821,15.942028985507241,16.666666666666661,17.391304347826082,18.115942028985504,18.840579710144926,19.565217391304348,20.289855072463769,21.014492753623191,21.739130434782613,22.463768115942035,23.188405797101456,23.913043478260878,24.6376811594203,25.362318840579722,26.086956521739143,26.811594202898565,27.536231884057987,28.260869565217408,28.98550724637683,29.710144927536252,30.434782608695674,31.159420289855095,31.884057971014517,32.608695652173935,33.333333333333357,34.057971014492779,34.7826086956522,35.507246376811622,36.231884057971044,36.956521739130466,37.681159420289887,38.405797101449309,39.130434782608731,39.855072463768153,40.579710144927574,41.304347826086996,42.028985507246418,42.75362318840584,43.478260869565261,44.202898550724683,44.927536231884105,45.652173913043526,46.376811594202948,47.10144927536237,47.826086956521792,48.550724637681213,49.275362318840635,50]],"y":[[0,22.064509648425339,39.731066072048677,52.852908948028897,62.274863684649333,69.144040335091077,74.442004699055886,78.534187834448758,81.64270770113265,83.98546257257081,85.737798441393025,87.050409975128844,88.072448633842185,88.901636351759649,89.566999068198228,90.092776773915801,90.503209459670231,90.822596633540499,91.077377614752379,91.296674782411714,91.509780428978715,91.745986846913624,92.033612389046795,92.370323284872825,92.71769888704749,93.035266362038058,93.296884115333597,93.51656008686345,93.715280046812396,93.914029765365228,94.133773947438385,94.385043536343957,94.651098965702531,94.910800562124592,95.143008652220601,95.326600558934558,95.446073755363244,95.499639911626062,95.487563227405062,95.410107902382236,95.267578945179437,95.069844041664552,94.848572319234151,94.638456358016924,94.474188738141493,94.390357875726977,94.403457338681676,94.491410779144388,94.627191418833846,94.783772479468766,94.934190599656333,95.059941476012924,95.159390026244864,95.23290225601248,95.280844170976096,95.303629405691765,95.306688823876939,95.304820063883611,95.313846077706913,95.349589817341979,95.427731610945372,95.551812363935738,95.704143919902108,95.864897581605305,96.014244651806109,96.132510205031522,96.210796871356791,96.257871351182217,96.284137706674414,96.299999999999997],[0,8.8556635460107067,17.5732556769591,26.014704977782859,34.041940033419671,41.516889428807218,48.301481748883191,54.257645578585269,59.248995955602993,63.240335082737971,66.353305268715459,68.723040444275654,70.48467454015875,71.773341487104958,72.724175215854459,73.472309657147449,74.146056167529764,74.794413678537509,75.415211815248938,76.005427380968015,76.562037178998708,77.082018012644966,77.562346685210741,78,78.393255295037491,78.74559204723117,79.061790268209791,79.346629969602091,79.604891163036825,79.84135386014276,80.060798072548607,80.267973569802905,80.465815596639459,80.654446884329388,80.833748227501843,81.003600420785943,81.163884258810853,81.314480536205707,81.455270047599655,81.586175586776719,81.707608187696437,81.820293877980021,81.924963935142983,82.022349636700895,82.113182260169268,82.198193083063671,82.278113382899619,82.35367443719268,82.425607523458382,82.49464391921228,82.561514901969886,82.626951749246771,82.691685738558462,82.756448147420514,82.821962429302488,82.888482594915928,82.955535018697361,83.022583482715604,83.089091769039484,83.154523659737791,83.218342936879367,83.280013382532985,83.339043704969541,83.39546487955873,83.449644828185697,83.501957088510792,83.552775198194396,83.602472694896889,83.651423116278636,83.700000000000003],[0,22.045641329259666,40.120778438814355,50.607016655088074,56.700926555855702,61.45978511145578,65.533709035228625,68.663073547122266,70.730994492229215,72.049766645169484,73.008425097912223,73.846766083196727,74.577344452009669,75.19363648180574,75.689159995624209,76.066240480438267,76.346854484733953,76.555637474411355,76.717224915370537,76.856252273511544,76.995815008479525,77.141945323152925,77.290052731223611,77.43538625723167,77.57339822862923,77.703443225750533,77.82839124542194,77.951237955685144,78.07497902458185,78.202610105053566,78.335123855512052,78.465967325531466,78.586811042763628,78.689325534860359,78.766287028167568,78.816830035726767,78.84235737282151,78.844274658441648,78.823987511577002,78.783056618509292,78.730782841947772,78.687642312519088,78.674982430571959,78.714064863854517,78.811873871368263,78.945268590286929,79.087287292170103,79.210968248577359,79.289349731068256,79.298412318725937,79.244511841190032,79.151923896078912,79.045155691224153,78.948021777000108,78.872133664620918,78.818669586137958,78.788471794347601,78.78238254204625,78.80124394011689,78.843404396589676,78.898363591178182,78.953659392291826,78.996829668340027,79.017381337471505,79.015471473009612,78.994841413029519,78.959235196634879,78.912396862929313,78.858070451016474,78.799999999999997],[0,23.378821650259848,37.621089542933234,45.836951100242523,51.717048048330327,55.841161759496316,58.730877441295071,60.814536868389105,62.268511077530079,63.22703001689294,63.824323634652636,64.194621878984123,64.471710791742382,64.742997599725641,65.009512472070682,65.262858680662021,65.494639497384142,65.696458194121576,65.860072358372136,65.983311570145503,66.071935620115937,66.132238582852381,66.170514532923747,66.193057544899006,66.206030954258708,66.212982935352642,66.215047273972246,66.213267251670885,66.208686150001952,66.202347250518827,66.195167440818153,66.186575992702444,66.175033670962463,66.15898470067259,66.136873306907191,66.107143714740616,66.068556546641361,66.022241690522179,65.970403155417756,65.915250284191671,65.858992419707462,65.803838904828737,65.751525362457912,65.701438221607503,65.65223705194137,65.602581207502141,65.551130042332389,65.496543082363061,65.438374309509626,65.379157300911004,65.322045297533236,65.270191540342367,65.226749270304424,65.194861423026524,65.175305799399666,65.163491802443389,65.154088064822162,65.141763219200428,65.121185898242658,65.087092170320304,65.038469730858253,64.98101724766579,64.921025047976627,64.864783459024466,64.818582808043018,64.788540510232153,64.775916870850395,64.776569098746108,64.786071904826812,64.799999999999997],[0,3.5767861858958927,7.1386775727038829,10.670779361336072,14.158196752704557,17.586034947721433,20.939399147298804,24.203394552348762,27.363126363783412,30.403699782514853,33.310220009455179,36.067792245516493,38.661521691610886,41.07651354865046,43.297873017547317,45.310705299213559,47.100115594561267,48.651209104502549,49.952307579946321,51.019728669921911,51.884204932703618,52.576588058047093,53.12772973570803,53.568481655442071,53.929695507004887,54.242222980152157,54.536904558072024,54.836455962506577,55.141146160471763,55.447400266326973,55.751643394431596,56.050300659145023,56.339797174826636,56.616558055835831,56.877008416531993,57.117673168945252,57.33737257153242,57.537222229177054,57.718437544433414,57.882233919855778,58.029826757998414,58.162431461415594,58.281263432661582,58.387538074290653,58.482504650667984,58.567610167287768,58.644373203442761,58.714312437148202,58.778946546419334,58.839794209271389,58.898374103719618,58.956204907779245,59.014799406618515,59.074957350918098,59.136093672312533,59.197464195567257,59.258324745447709,59.317931146719296,59.375539224147467,59.430404802497641,59.481783706535253,59.528983317990253,59.572010955943128,59.611378372815338,59.647608457332694,59.681224098221008,59.712748184206085,59.742703604013741,59.771613246369768,59.799999999999997],[0,23.846762050857318,34.213972741731702,40.149555899292103,43.342744162908353,45.008514189927311,45.903761465855716,46.499524669042373,46.868117180272741,47.054162631294858,47.102284653856749,47.057106879706446,46.963252940591985,46.864897365541026,46.786259257737058,46.724090365226822,46.67314270711352,46.62816830250032,46.583919170490425,46.535147330187009,46.476604800693259,46.403043601112365,46.310489357081792,46.200653587612123,46.076833925719846,45.942328074167207,45.800433735716446,45.654448613129809,45.507670409169535,45.363396826597878,45.224810119065076,45.092959176193297,44.967014602450867,44.846082828436465,44.729270284748779,44.615683401986495,44.504428610748292,44.394612341632865,44.285341496026092,44.176005600791463,44.066754634289353,43.957865171362769,43.849613786854739,43.742277055608263,43.63613155246636,43.531453852272051,43.428520529868337,43.327577783249708,43.228578703751097,43.131312360977745,43.035566024958911,42.941126965723846,42.847782453301818,42.755319757722077,42.663526149013883,42.57219575471764,42.481632920074865,42.39299554616575,42.307522811706441,42.226453895413066,42.151027976001764,42.082484232188669,42.022061842689929,41.970905631962601,41.928699747032674,41.893978378249741,41.865244622384409,41.841001576207269,41.819752336488932,41.799999999999997],[0,1.485361963107545,2.9632012226730953,4.4259950751546571,5.8662208170102348,7.2763557446978355,8.6488771546754624,9.9762623434011228,11.250988607332824,12.466063127563039,13.621383130285585,14.721664238705714,15.771720946631035,16.776367747869152,17.740419136227668,18.668689605514196,19.565993649536342,20.437145762101711,21.286727968788487,22.115486620228026,22.921021255898861,23.70083841443078,24.45244463445357,25.173346454597016,25.861050413490908,26.51306304976503,27.126899862764322,27.701712479147822,28.240181297001886,28.745445879222107,29.220645788704076,29.668920588343383,30.093409841035623,30.497253109676382,30.883589957161256,31.255557740410733,31.615334270121174,31.962641259610663,32.296813017674509,32.617183853108031,32.92308807470652,33.213859991265309,33.48883391157969,33.747344144444988,33.988815354593328,34.213366609815928,34.421438940330667,34.613475139673966,34.78991800138224,34.951210318991897,35.097794886039352,35.230114496061013,35.348626091914333,35.454265378122372,35.548551625884755,35.633039474547253,35.709283563455621,35.778838531955635,35.843259019393059,35.904099665113655,35.962915108463193,36.021247032801249,36.08000571959797,36.139198580035938,36.198763589309266,36.258638722612055,36.318761955138413,36.379071262082455,36.439504618638281,36.5],[0,8.5499314169564489,15.459906045895737,20.373043949396532,24.317694574607092,27.460998151719476,29.867702349416611,31.626788535089112,32.852769860294501,33.661376674095166,34.168339325553518,34.489388163731945,34.723933796633105,34.897776819651291,35.015973435103412,35.083578664769554,35.105647530429813,35.087294315714139,35.035473582824473,34.959292332436654,34.867979739919313,34.770720215126197,34.673234643446257,34.575372995893211,34.476416555643816,34.375646605874813,34.272344429762953,34.165791310484984,34.055289869105266,33.940972237068813,33.824048109144748,33.705799195472842,33.587507206192875,33.470453851444624,33.355920841367876,33.245147449312455,33.138396902459291,33.034956381820436,32.934070631617971,32.834984396073985,32.736942419410568,32.639189445849809,32.540994272465547,32.441985598261496,32.342069175459642,32.241157883052871,32.139164600034071,32.036002205396137,31.931583578131939,31.825889674777539,31.719604258225754,31.613825709409287,31.509657768134513,31.4082041742078,31.310568667435518,31.217854987624033,31.131015091320691,31.049879161924039,30.973774600787099,30.902026437649454,30.833959702250706,30.768899424330439,30.706170633628247,30.645152388202,30.585515973350955,30.52703102221848,30.469467242060862,30.412594340134383,30.356182023695332,30.299999999999997],[0,1.1454423775641578,2.2862123937423506,3.417637687148614,4.5350458963969826,5.6337646601014928,6.7091216168761783,7.7564444053350758,8.7710606640922197,9.7482980317616441,10.683484146957387,11.57218038838599,12.412836532465196,13.205850473425178,13.95165659746322,14.650886066411056,15.30849024269194,15.93362944257597,16.5356378246052,17.120106813245116,17.680114709812305,18.20612783409474,18.689509916552481,19.134534870524202,19.555156578760673,19.965547403122486,20.373827847795145,20.77299892900384,21.153739272308325,21.506727526948669,21.825783465104788,22.116559984141588,22.387495946977282,22.646332570765573,22.889023272839083,23.102155287797931,23.282403770988253,23.436831311560461,23.572952126221658,23.698280431678967,23.820330444639499,23.946616381810365,24.084190538339019,24.233193494183908,24.388445177264412,24.544628649852601,24.696426974220554,24.838523212640347,24.96560042738405,25.072805409181093,25.160072302893511,25.230159535445768,25.285862037168584,25.329974738392679,25.365292569448776,25.394610460667604,25.420501203542397,25.443895844720657,25.464989595950737,25.483974198061652,25.501041391882417,25.516382918242044,25.530190517969555,25.542655931893957,25.55397090084427,25.564327165649505,25.573916467138684,25.582930546140815,25.591561143484917,25.600000000000001],[0,5.340293111192655,9.5867429476451438,13.036117879725834,15.526408971911778,17.285570006282835,18.576381550865314,19.556845751300287,20.274573842705482,20.771914304569361,21.091144975727474,21.270501793005081,21.342066214410931,21.337402984511243,21.288035437278889,21.216707860898165,21.126577332902411,21.018150652851052,20.891934966943236,20.750347393371609,20.602190680265817,20.457549429915993,20.322556301228271,20.196645134763784,20.07860088808668,19.967208518761094,19.861252984351175,19.759519242421071,19.660790605776597,19.5637864472438,19.467143079353448,19.369491263576982,19.269461761385831,19.165685334251432,19.056792743645214,18.9415065920203,18.820661824408482,18.697205728420247,18.574177432647762,18.454616065683187,18.341560756118685,18.238050632546429,18.146890079491985,18.067371014706801,17.996081452064193,17.929539851639987,17.864264673509997,17.796774377750047,17.723587424435948,17.641626032384142,17.551980670266818,17.458200850514618,17.363867868316195,17.272563018860193,17.18786759733527,17.11336289893007,17.052022713757776,17.002330989733174,16.960759314208563,16.923769782269435,16.887824489001282,16.849385529489599,16.804914998819871,16.75147958330551,16.689416069687439,16.620161783196906,16.545154878408404,16.46583350989642,16.383635832235452,16.299999999999994]],"xo":[[0,0.10000000000000001,0.20000000000000001,0.29999999999999999,1,3,5,7,10,13,15,18,21,24,27,30,33,36,39,41.600000000000001],[0,2.2999999999999998,4.5999999999999996,6.9000000000000004,9.1999999999999993,11.5,16.100000000000001,18.399999999999999,20.699999999999999],[0,0.10000000000000001,0.20000000000000001,0.29999999999999999,1,3,5,7,10,14,17,21,24,28,31,35,38,42,45,50],[0,0.10000000000000001,0.20000000000000001,0.29999999999999999,0.5,0.80000000000000004,1,2,5,10,15,20,25,30,35,40,45,50,55,58.799999999999997],[0,4,6,8,10,12,14,16],[0,0.10000000000000001,0.20000000000000001,0.29999999999999999,0.5,0.80000000000000004,1,2,3,4,5,8,18,30,42,54,66,78,89,98.400000000000006],[0,1.2,2.5,3.7000000000000002,5,6.2000000000000002,7.4000000000000004,8.6999999999999993,9.9000000000000004],[0,0.10000000000000001,0.20000000000000001,0.29999999999999999,0.40000000000000002,0.59999999999999998,0.80000000000000004,1,2,4,8,12,15,20,25,30,35,40,45,50],[0,1.5,2.1000000000000001,2.6000000000000001,3.1000000000000001,3.6000000000000001,4.2000000000000002,4.7000000000000002,5,6,7,8,10],[0,0.10000000000000001,0.20000000000000001,0.40000000000000002,0.5,0.69999999999999996,1,2,4,7,10,13,15,20,25,30,35,40,45,50]],"yo":[[0,5.5,9,12.199999999999999,34.200000000000003,69,82.400000000000006,87.700000000000003,90.700000000000003,91.900000000000006,93,94.099999999999994,95.299999999999997,95.299999999999997,94.400000000000006,94.900000000000006,95.299999999999997,95.400000000000006,96.099999999999994,96.299999999999997],[0,57.700000000000003,73.700000000000003,78,80.200000000000003,81.5,82.799999999999997,83.299999999999997,83.700000000000003],[0,3.6000000000000001,7.5,10.199999999999999,29.899999999999999,57.399999999999999,68.400000000000006,72.700000000000003,75.599999999999994,76.900000000000006,77.5,78.200000000000003,78.700000000000003,78.799999999999997,78.700000000000003,79.299999999999997,79,78.799999999999997,79,78.799999999999997],[0,3.7999999999999998,6.9000000000000004,9.9000000000000004,15.199999999999999,22.199999999999999,26.600000000000001,40.799999999999997,58.399999999999999,64.400000000000006,65.799999999999997,66.200000000000003,66.200000000000003,66.099999999999994,65.799999999999997,65.5,65.200000000000003,65.099999999999994,64.799999999999997,64.799999999999997],[0,49,54.5,57,58.399999999999999,59,59.5,59.799999999999997],[0,4.0999999999999996,5.0999999999999996,6.2999999999999998,11.5,15.1,18.300000000000001,28.300000000000001,35.100000000000001,39.299999999999997,42,45.600000000000001,46.899999999999999,46.399999999999999,45.299999999999997,44.299999999999997,43.399999999999999,42.600000000000001,42,41.799999999999997],[0,11.699999999999999,20.800000000000001,27,31.199999999999999,33.799999999999997,35.299999999999997,36,36.5],[0,1.8,3,4.2000000000000002,5,7.0999999999999996,9.4000000000000004,11.5,19.300000000000001,28.800000000000001,34.5,35.100000000000001,34.799999999999997,34.100000000000001,33.299999999999997,32.600000000000001,31.899999999999999,31.199999999999999,30.699999999999999,30.300000000000001],[0,11,14.300000000000001,16.5,18.399999999999999,19.899999999999999,21.5,22.5,23,24,25,25.399999999999999,25.600000000000001],[0,1,1.8,3,3.8999999999999999,5.2000000000000002,7,12.300000000000001,18,21,21.300000000000001,20.899999999999999,20.5,19.699999999999999,19,18.199999999999999,17.699999999999999,17.100000000000001,16.800000000000001,16.300000000000001]],"z":[{"value":-40,"unit":"\u00b0C","name":"","comment":null,"realZ":-40},{"value":-20,"unit":"\u00b0C","name":"","comment":null,"realZ":-20},{"value":0,"unit":"\u00b0C","name":"","comment":null,"realZ":0},{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23},{"value":40,"unit":"\u00b0C","name":"","comment":null,"realZ":40},{"value":60,"unit":"\u00b0C","name":"","comment":null,"realZ":60},{"value":80,"unit":"\u00b0C","name":"","comment":null,"realZ":80},{"value":90,"unit":"\u00b0C","name":"","comment":null,"realZ":90},{"value":100,"unit":"\u00b0C","name":"","comment":null,"realZ":100},{"value":120,"unit":"\u00b0C","name":"","comment":null,"realZ":120}],"zo":[{"value":-40,"unit":"\u00b0C","name":"","comment":null,"realZ":-40},{"value":-20,"unit":"\u00b0C","name":"","comment":null,"realZ":-20},{"value":0,"unit":"\u00b0C","name":"","comment":null,"realZ":0},{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23},{"value":40,"unit":"\u00b0C","name":"","comment":null,"realZ":40},{"value":60,"unit":"\u00b0C","name":"","comment":null,"realZ":60},{"value":80,"unit":"\u00b0C","name":"","comment":null,"realZ":80},{"value":90,"unit":"\u00b0C","name":"","comment":null,"realZ":90},{"value":100,"unit":"\u00b0C","name":"","comment":null,"realZ":100},{"value":120,"unit":"\u00b0C","name":"","comment":null,"realZ":120}],"keys":["Y - Yield"],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"P","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"stress-strain-delrin\u00ae-100p-nc010.png","svgname":"stress-strain-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","Y","","","Y","","Y","","Y",""],"xmarker":[],"option":1},"moist":0,"name":"Stress-strain","shortname":"&#963; &#949;"},{"id":4,"addId":[],"data":{"name":"Secant modulus-strain ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"P","axes":{"x":{"name":"Strain in","unit":"%","log":false},"y":{"name":"Secant modulus in","unit":"MPa","log":false},"z":{"name":"","unit":"\u00b0C"}},"x":[[0.10000000000000001,0.70144927536231882,1.3028985507246378,1.9043478260869566,2.5057971014492755,3.1072463768115943,3.7086956521739132,4.310144927536232,4.9115942028985504,5.5130434782608688,6.1144927536231872,6.7159420289855056,7.317391304347824,7.9188405797101424,8.5202898550724608,9.1217391304347792,9.7231884057970976,10.324637681159416,10.926086956521734,11.527536231884053,12.128985507246371,12.73043478260869,13.331884057971008,13.933333333333326,14.534782608695645,15.136231884057963,15.737681159420282,16.3391304347826,16.94057971014492,17.54202898550724,18.143478260869561,18.744927536231881,19.346376811594201,19.947826086956521,20.549275362318841,21.150724637681162,21.752173913043482,22.353623188405802,22.955072463768122,23.556521739130442,24.157971014492762,24.759420289855083,25.360869565217403,25.962318840579723,26.563768115942043,27.165217391304363,27.766666666666683,28.368115942029004,28.969565217391324,29.571014492753644,30.172463768115964,30.773913043478284,31.375362318840605,31.976811594202925,32.578260869565241,33.179710144927562,33.781159420289882,34.382608695652202,34.984057971014522,35.585507246376842,36.186956521739162,36.788405797101483,37.389855072463803,37.991304347826123,38.592753623188443,39.194202898550763,39.795652173913084,40.397101449275404,40.998550724637724,41.600000000000001],[2.2999999999999998,2.5666666666666664,2.833333333333333,3.0999999999999996,3.3666666666666663,3.6333333333333329,3.8999999999999995,4.1666666666666661,4.4333333333333327,4.6999999999999993,4.9666666666666659,5.2333333333333325,5.4999999999999991,5.7666666666666657,6.0333333333333323,6.2999999999999989,6.5666666666666655,6.8333333333333321,7.0999999999999988,7.3666666666666654,7.633333333333332,7.8999999999999986,8.1666666666666661,8.4333333333333336,8.7000000000000011,8.9666666666666686,9.2333333333333361,9.5000000000000036,9.766666666666671,10.033333333333339,10.300000000000006,10.566666666666674,10.833333333333341,11.100000000000009,11.366666666666676,11.633333333333344,11.900000000000011,12.166666666666679,12.433333333333346,12.700000000000014,12.966666666666681,13.233333333333348,13.500000000000016,13.766666666666683,14.033333333333351,14.300000000000018,14.566666666666686,14.833333333333353,15.100000000000021,15.366666666666688,15.633333333333356,15.900000000000023,16.166666666666689,16.433333333333355,16.700000000000021,16.966666666666686,17.233333333333352,17.500000000000018,17.766666666666683,18.033333333333349,18.300000000000015,18.566666666666681,18.833333333333346,19.100000000000012,19.366666666666678,19.633333333333344,19.900000000000009,20.166666666666675,20.433333333333341,20.699999999999999],[0.10000000000000001,0.8231884057971014,1.5463768115942029,2.2695652173913041,2.9927536231884053,3.7159420289855065,4.4391304347826077,5.1623188405797089,5.8855072463768101,6.6086956521739113,7.3318840579710125,8.0550724637681146,8.7782608695652158,9.501449275362317,10.224637681159418,10.947826086956519,11.671014492753621,12.394202898550722,13.117391304347823,13.840579710144924,14.563768115942025,15.286956521739127,16.010144927536228,16.733333333333331,17.456521739130434,18.179710144927537,18.90289855072464,19.626086956521743,20.349275362318846,21.072463768115949,21.795652173913052,22.518840579710155,23.242028985507257,23.96521739130436,24.688405797101463,25.411594202898566,26.134782608695669,26.857971014492772,27.581159420289875,28.304347826086978,29.027536231884081,29.750724637681184,30.473913043478287,31.19710144927539,31.920289855072493,32.643478260869593,33.366666666666696,34.089855072463799,34.813043478260902,35.536231884058004,36.259420289855107,36.98260869565221,37.705797101449313,38.428985507246416,39.152173913043519,39.875362318840622,40.598550724637725,41.321739130434828,42.044927536231931,42.768115942029034,43.491304347826137,44.21449275362324,44.937681159420343,45.660869565217446,46.384057971014549,47.107246376811652,47.830434782608755,48.553623188405858,49.276811594202961,50],[0.10000000000000001,0.95072463768115933,1.8014492753623186,2.652173913043478,3.5028985507246375,4.3536231884057965,5.2043478260869556,6.0550724637681146,6.9057971014492736,7.7565217391304326,8.6072463768115917,9.4579710144927507,10.30869565217391,11.159420289855069,12.010144927536228,12.860869565217387,13.711594202898546,14.562318840579705,15.413043478260864,16.263768115942025,17.114492753623185,17.965217391304346,18.815942028985507,19.666666666666668,20.517391304347829,21.368115942028989,22.21884057971015,23.069565217391311,23.920289855072472,24.771014492753633,25.621739130434793,26.472463768115954,27.323188405797115,28.173913043478276,29.024637681159437,29.875362318840597,30.726086956521758,31.576811594202919,32.427536231884076,33.278260869565237,34.128985507246398,34.979710144927559,35.83043478260872,36.68115942028988,37.531884057971041,38.382608695652202,39.233333333333363,40.084057971014524,40.934782608695684,41.785507246376845,42.636231884058006,43.486956521739167,44.337681159420328,45.188405797101488,46.039130434782649,46.88985507246381,47.740579710144971,48.591304347826132,49.442028985507292,50.292753623188453,51.143478260869614,51.994202898550775,52.844927536231936,53.695652173913096,54.546376811594257,55.397101449275418,56.247826086956579,57.09855072463774,57.9492753623189,58.799999999999997],[4,4.1739130434782608,4.3478260869565215,4.5217391304347823,4.695652173913043,4.8695652173913038,5.0434782608695645,5.2173913043478253,5.391304347826086,5.5652173913043468,5.7391304347826075,5.9130434782608683,6.086956521739129,6.2608695652173898,6.4347826086956506,6.6086956521739113,6.7826086956521721,6.9565217391304328,7.1304347826086936,7.3043478260869543,7.4782608695652151,7.6521739130434758,7.8260869565217366,7.9999999999999973,8.1739130434782581,8.3478260869565197,8.5217391304347814,8.695652173913043,8.8695652173913047,9.0434782608695663,9.2173913043478279,9.3913043478260896,9.5652173913043512,9.7391304347826129,9.9130434782608745,10.086956521739136,10.260869565217398,10.434782608695659,10.608695652173921,10.782608695652183,10.956521739130444,11.130434782608706,11.304347826086968,11.478260869565229,11.652173913043491,11.826086956521753,12.000000000000014,12.173913043478276,12.347826086956537,12.521739130434799,12.695652173913061,12.869565217391322,13.043478260869584,13.217391304347846,13.391304347826107,13.565217391304369,13.739130434782631,13.913043478260892,14.086956521739154,14.260869565217416,14.434782608695677,14.608695652173939,14.7826086956522,14.956521739130462,15.130434782608724,15.304347826086985,15.478260869565247,15.652173913043509,15.82608695652177,16],[0.10000000000000001,1.5246376811594204,2.9492753623188408,4.3739130434782609,5.7985507246376811,7.2231884057971012,8.6478260869565222,10.072463768115943,11.497101449275364,12.921739130434785,14.346376811594206,15.771014492753627,17.195652173913047,18.620289855072468,20.044927536231889,21.46956521739131,22.894202898550731,24.318840579710152,25.743478260869573,27.168115942028994,28.592753623188415,30.017391304347836,31.442028985507257,32.866666666666674,34.291304347826092,35.715942028985509,37.140579710144927,38.565217391304344,39.989855072463762,41.414492753623179,42.839130434782597,44.263768115942014,45.688405797101431,47.113043478260849,48.537681159420266,49.962318840579684,51.386956521739101,52.811594202898519,54.236231884057936,55.660869565217354,57.085507246376771,58.510144927536189,59.934782608695606,61.359420289855024,62.784057971014441,64.208695652173859,65.633333333333283,67.057971014492708,68.482608695652132,69.907246376811557,71.331884057970981,72.756521739130406,74.181159420289831,75.605797101449255,77.03043478260868,78.455072463768104,79.879710144927529,81.304347826086953,82.728985507246378,84.153623188405803,85.578260869565227,87.002898550724652,88.427536231884076,89.852173913043501,91.276811594202925,92.70144927536235,94.126086956521775,95.550724637681199,96.975362318840624,98.400000000000006],[1.2,1.326086956521739,1.4521739130434781,1.5782608695652172,1.7043478260869562,1.8304347826086953,1.9565217391304344,2.0826086956521737,2.2086956521739127,2.3347826086956518,2.4608695652173909,2.5869565217391299,2.713043478260869,2.8391304347826081,2.9652173913043471,3.0913043478260862,3.2173913043478253,3.3434782608695643,3.4695652173913034,3.5956521739130425,3.7217391304347816,3.8478260869565206,3.9739130434782597,4.0999999999999988,4.2260869565217378,4.3521739130434769,4.478260869565216,4.604347826086955,4.7304347826086941,4.8565217391304332,4.9826086956521722,5.1086956521739113,5.2347826086956504,5.3608695652173894,5.4869565217391285,5.6130434782608676,5.7391304347826066,5.8652173913043457,5.9913043478260848,6.1173913043478239,6.2434782608695629,6.369565217391302,6.4956521739130411,6.6217391304347801,6.7478260869565192,6.8739130434782583,6.9999999999999973,7.1260869565217364,7.2521739130434755,7.3782608695652145,7.5043478260869536,7.6304347826086927,7.7565217391304317,7.8826086956521708,8.0086956521739108,8.1347826086956498,8.2608695652173889,8.386956521739128,8.513043478260867,8.6391304347826061,8.7652173913043452,8.8913043478260843,9.0173913043478233,9.1434782608695624,9.2695652173913015,9.3956521739130405,9.5217391304347796,9.6478260869565187,9.7739130434782577,9.8999999999999968],[0.10000000000000001,0.8231884057971014,1.5463768115942029,2.2695652173913041,2.9927536231884053,3.7159420289855065,4.4391304347826077,5.1623188405797089,5.8855072463768101,6.6086956521739113,7.3318840579710125,8.0550724637681146,8.7782608695652158,9.501449275362317,10.224637681159418,10.947826086956519,11.671014492753621,12.394202898550722,13.117391304347823,13.840579710144924,14.563768115942025,15.286956521739127,16.010144927536228,16.733333333333331,17.456521739130434,18.179710144927537,18.90289855072464,19.626086956521743,20.349275362318846,21.072463768115949,21.795652173913052,22.518840579710155,23.242028985507257,23.96521739130436,24.688405797101463,25.411594202898566,26.134782608695669,26.857971014492772,27.581159420289875,28.304347826086978,29.027536231884081,29.750724637681184,30.473913043478287,31.19710144927539,31.920289855072493,32.643478260869593,33.366666666666696,34.089855072463799,34.813043478260902,35.536231884058004,36.259420289855107,36.98260869565221,37.705797101449313,38.428985507246416,39.152173913043519,39.875362318840622,40.598550724637725,41.321739130434828,42.044927536231931,42.768115942029034,43.491304347826137,44.21449275362324,44.937681159420343,45.660869565217446,46.384057971014549,47.107246376811652,47.830434782608755,48.553623188405858,49.276811594202961,50],[1.5,1.6231884057971016,1.7463768115942031,1.8695652173913047,1.9927536231884062,2.1159420289855078,2.2391304347826093,2.3623188405797109,2.4855072463768124,2.608695652173914,2.7318840579710155,2.8550724637681171,2.9782608695652186,3.1014492753623202,3.2246376811594217,3.3478260869565233,3.4710144927536248,3.5942028985507264,3.7173913043478279,3.8405797101449295,3.963768115942031,4.0869565217391326,4.2101449275362341,4.3333333333333357,4.4565217391304373,4.5797101449275388,4.7028985507246404,4.8260869565217419,4.9492753623188435,5.072463768115945,5.1956521739130466,5.3188405797101481,5.4420289855072497,5.5652173913043512,5.6884057971014528,5.8115942028985543,5.9347826086956559,6.0579710144927574,6.181159420289859,6.3043478260869605,6.4275362318840621,6.5507246376811636,6.6739130434782652,6.7971014492753667,6.9202898550724683,7.0434782608695699,7.1666666666666714,7.289855072463773,7.4130434782608745,7.5362318840579761,7.6594202898550776,7.7826086956521792,7.9057971014492807,8.0289855072463823,8.1521739130434838,8.2753623188405854,8.3985507246376869,8.5217391304347885,8.64492753623189,8.7681159420289916,8.8913043478260931,9.0144927536231947,9.1376811594202962,9.2608695652173978,9.3840579710144993,9.5072463768116009,9.6304347826087024,9.753623188405804,9.8768115942029056,10],[0.10000000000000001,0.8231884057971014,1.5463768115942029,2.2695652173913041,2.9927536231884053,3.7159420289855065,4.4391304347826077,5.1623188405797089,5.8855072463768101,6.6086956521739113,7.3318840579710125,8.0550724637681146,8.7782608695652158,9.501449275362317,10.224637681159418,10.947826086956519,11.671014492753621,12.394202898550722,13.117391304347823,13.840579710144924,14.563768115942025,15.286956521739127,16.010144927536228,16.733333333333331,17.456521739130434,18.179710144927537,18.90289855072464,19.626086956521743,20.349275362318846,21.072463768115949,21.795652173913052,22.518840579710155,23.242028985507257,23.96521739130436,24.688405797101463,25.411594202898566,26.134782608695669,26.857971014492772,27.581159420289875,28.304347826086978,29.027536231884081,29.750724637681184,30.473913043478287,31.19710144927539,31.920289855072493,32.643478260869593,33.366666666666696,34.089855072463799,34.813043478260902,35.536231884058004,36.259420289855107,36.98260869565221,37.705797101449313,38.428985507246416,39.152173913043519,39.875362318840622,40.598550724637725,41.321739130434828,42.044927536231931,42.768115942029034,43.491304347826137,44.21449275362324,44.937681159420343,45.660869565217446,46.384057971014549,47.107246376811652,47.830434782608755,48.553623188405858,49.276811594202961,50]],"y":[[5500,3493.7371833020047,3334.4552998916029,3019.6628158217704,2614.4037653629989,2241.1188250097644,1978.3221369947582,1800.3492139299351,1666.4303906008431,1540.6372953588154,1417.3048254329879,1302.4386869373118,1201.8537664041096,1116.9965504182494,1045.249834830674,983.84186678470701,930.0008934236721,881.02893284461834,835.64547192241503,793.84775448110634,755.67875858246066,721.18146228824708,690.37681976172416,662.88405079193626,637.97146260637089,614.89701725811506,593.14402832953567,572.66278726613427,553.46156894140358,535.54864822883656,518.93184480689888,503.55709299555974,489.24628955227877,475.80652811747007,463.04490233154803,450.76898335814764,438.84377896472631,427.24566296118746,415.96377870894241,404.98726956940271,394.30559217935024,383.9417549924558,373.981709186285,364.5183371800174,355.64452139283242,347.45239277200488,339.96200107337029,333.06254385523255,326.62938627138084,320.53789347560422,314.66391776932437,308.92538219902417,303.3141244069343,297.82947916189761,292.47078123275702,287.23750546143299,282.14007058397152,277.20750640553837,272.47065310646155,267.96035086706922,263.70702005497054,259.71127677751394,255.92467090470856,252.29417737543534,248.76677112857519,245.28970623549441,241.82831633837162,238.37675215974807,234.93173846012405,231.48999999999978],[2508.6999999999998,2391.8338576815154,2275.9292453771641,2161.9476931010804,2050.8507308673966,1943.5998886902471,1841.1566965837651,1744.4826845620839,1654.5393826393374,1572.273350330657,1497.9530389926908,1430.9059763966854,1370.3903824481381,1315.6644770525463,1265.9864801154081,1220.6146115422202,1178.8070912384812,1139.8221391096879,1102.965351239797,1067.9546719326868,1034.7203609586627,1003.1944327613065,973.30890178419986,944.99578247092472,918.18708926506292,892.81483661019627,868.81103369306334,846.1038784890842,824.61103951675329,804.24838219734784,784.9317719521456,766.57707420242377,749.1001543694598,732.41687787453134,716.4431101389157,701.09606767414323,686.32404206755757,672.10639998231636,658.42385917183003,645.25713738950867,632.58695238876271,620.39402192300247,608.65906374563815,597.36279561008007,586.48593526973855,576.0092004780239,565.91330898834644,556.17897855411638,546.78692692874415,537.71787186563984,528.95253111821398,520.4716224398768,512.25589954773909,504.29046776666178,496.56888389110384,489.08567573543542,481.83537111402671,474.81249784124788,468.01158373146905,461.42715659906037,455.05374425839204,448.88513718170969,442.90511568457708,437.09024592721204,431.41693480393349,425.8615892090603,420.4006160369114,415.01042218180578,409.6674145380623,404.3479999999999],[3600,2832.3794294488748,3114.8378138993776,2610.5722691412079,1919.0818089009611,1534.9782188617014,1408.8817899621283,1351.7016789332654,1243.4544930794018,1108.1823122363971,987.10802797187876,898.29990424257994,834.05087703151821,785.30467333814011,743.05396569363506,701.77228529547403,661.66706423140636,623.480783253504,587.95592311383916,555.83496456448393,527.74074364511216,503.35141734390368,481.89687535193377,462.60430201462316,444.732123811073,427.95291470867437,412.23281352632489,397.54418584818541,383.85939725841706,371.15079652191139,359.36853511912216,348.39684698874322,338.10778638223354,328.37340755105197,319.08165642407266,310.19392648461888,301.69281562030551,293.56092376859993,285.78085086696956,278.33586024768721,271.23209178566765,264.50381954169802,258.18704662719585,252.31733582931656,246.88719069410399,241.81048775120112,236.99273063291713,232.33942297156128,227.75606839944271,223.15906525216045,218.5623793736346,214.03140051841316,209.63198016176582,205.42727002587833,201.43891499109316,197.65603020836303,194.0668599913329,190.65964865364771,187.42263996986151,184.34138582769918,181.39249485969947,178.5507208240121,175.79081747878678,173.08974792629701,170.43593242021493,167.82149374233242,165.23855652700956,162.67924540860645,160.13568502148314,157.59999999999977],[3800,2687.468200435258,2159.6035246894785,1718.5773510739132,1438.0840978281051,1263.6601339904146,1140.0772546611679,1029.3405628066068,927.83924177505128,836.04367152383395,754.42423201028828,683.45130319174712,623.57745085524903,574.3826610082275,534.19661436456158,501.25255510350712,473.78372740432042,450.02337544625732,428.23969023542656,407.56204906960255,388.01417112380523,369.66135648376564,352.5689052352148,336.80211746388369,322.4180217889957,309.35380228676837,297.45635166309842,286.57035074483241,276.54048035881664,267.21142133189755,258.43618774042136,250.14515454828401,242.31067416260697,234.90551529756544,227.90244666733446,221.27423698608919,214.99446238068452,209.04173863346341,203.39662235669948,198.03967424659118,192.9514549993369,188.11252531113519,183.50417553730728,179.1108312252525,174.9177598167449,170.91022876420095,167.07350552003712,163.39285970472542,159.85653397775457,156.46163587103612,153.20691786933341,150.0911324574096,147.11303212002801,144.27134219303943,141.56034169745854,138.96496611312378,136.46897149310678,134.05611389047917,131.71014935831258,129.41501970735138,127.16499310697874,124.96988956515467,122.84081519014499,120.78887609021557,118.82517837363218,116.9602404139065,115.18869512235896,113.48785142058647,111.83414211199732,110.20399999999987],[1225,1195.0364229346719,1165.183808895436,1135.553120908384,1106.255321999608,1077.4013751952002,1049.1022435212524,1021.4688900038567,994.61227766910508,968.64336954308965,943.67312865190229,919.81251802163501,897.16856158967209,875.75768425311855,855.5057118688004,836.33453120483546,818.16602902934187,800.92209211043757,784.52460721624084,768.89546111486948,753.95654057444176,739.62973236307562,725.83692324888898,712.50000000000023,699.55227213079536,686.97274014073389,674.75182727554363,662.87995678095228,651.34755190268754,640.14503588647722,629.26283197804901,618.6913634231305,608.42105346744961,598.44232535673393,588.74560233671127,579.32137107181438,570.1615768566927,561.25962361621248,552.60897869394478,544.20310943346078,536.0354831783319,528.09956727212909,520.38882905842365,512.89673588078676,505.61675508278961,498.54235400800343,491.6669999999994,484.98429583046135,478.48838598352353,472.17355037143284,466.03406890643606,460.06422150078015,454.258288066712,448.61054851647839,443.11528276232622,437.76677071650238,432.55929229125377,427.48712739882717,422.54444553046955,417.72287649442626,413.01151041594159,408.39932699925964,403.87530594862454,399.42842696828046,395.04766976247157,390.72201403544193,386.44043949143577,382.19192583469714,377.96545276947029,373.7499999999992],[4100,1678.8691150563825,1178.0410571393127,922.05627967156784,752.08689789499044,625.935010932458,528.5335456480824,451.78706729756243,392.46822365047734,347.60915029470073,314.24198281810612,289.3988568085669,270.11190785395689,253.4542105062408,237.80193642729637,223.07384876469098,209.27797634061926,196.42234797727582,184.51499249685529,173.56393872155223,163.57721547356127,154.5628515431973,146.51070227092674,139.34054281404221,132.95525836008972,127.25773409661535,122.15085521116519,117.53750689128532,113.32057432452183,109.40294269842076,105.69073761813682,102.14074517420273,98.749892807562873,95.516208761612049,92.437721279745006,89.512458605356514,86.738448981841373,84.113720652594338,81.63629580091316,79.30211479107713,77.102002445250619,75.02601204582021,73.064196875172499,71.206610215694042,69.443305349771464,67.76433555979132,66.159754128140207,64.620126038717459,63.140581277002987,61.718648347712843,60.351877057038408,59.037817211171074,57.774018616302229,56.558031078623259,55.387404404325565,54.259701353922047,53.173345817828917,52.128147036549258,51.124039537029638,50.160957846216618,49.238836491056738,48.357609998496571,47.517212895482672,46.717361806471317,45.954489126343056,45.222486834787361,44.515180854089721,43.826397106535616,43.149961514410542,42.47969999999998],[975,960.27364320037566,945.59610494551134,931.01620378016707,916.58275824910288,902.3445868970789,888.35050826885492,874.6493409091911,861.28990336284755,848.32101417458409,835.79149188916097,823.74386031106428,812.15325096856782,800.95391419923749,790.07952673243187,779.46376529750955,769.04030662382911,758.74282744074912,748.50500447762818,738.26051446382485,727.94312730626962,717.51553821187383,707.01019959035079,696.46986854543866,685.93730218087535,675.45525760039891,665.06649190774749,654.81376220665925,644.739825600872,634.887439194124,625.29936009015319,616.01113349580532,607.0144729010301,598.28462282342446,589.79679824065533,581.5262141303898,573.4480854702947,565.53762723803732,557.77005441128438,550.12058196770306,542.56460198901812,535.08730377632173,527.68860389572717,520.36963367007968,513.13152442222463,505.97540747500693,498.90241415127201,491.91367577386495,485.01032366563095,478.1934891494152,471.46511461354459,464.83263292079914,458.30575359664346,451.89419350039515,445.60766949137189,439.45589842889149,433.44859717227149,427.59548258082964,421.90627151388361,416.39068083075102,411.05774762488716,405.90207096424143,400.90444694363197,396.04511898305418,391.30433050250366,386.66232492197577,382.09934566146597,377.59563614096982,373.13143978048271,368.68700000000013],[1800,1172.4464075441886,1053.6302777732201,918.47186716242538,819.43629078366939,745.56010944830143,681.75204513124197,621.72649889545028,565.84895678262251,514.64878627435371,468.65535485223847,428.39792444269568,394.10829215904687,365.0701835884704,340.37885896653722,319.12957852881834,300.41760251088465,283.36241563009168,267.53831475482133,252.92390956460446,239.51189047493313,227.29382484089129,216.21678243504013,206.16953921379118,197.03692558826449,188.70377196958012,181.05490876885807,173.97516639721835,167.35119793895035,161.11513162273116,155.2466373345687,149.72762119212575,144.53998931306495,139.66564781504903,135.08650281574069,130.78440123037839,126.74018607540116,122.93386235147813,119.34540937307902,115.9548064546736,112.7420329107316,109.68706805572276,106.77053184463459,103.98080717502975,101.31143929244735,98.756066672598493,96.308327791194245,93.96186112394571,91.710305146563968,89.547578433638634,87.470107985086173,85.475642890953722,83.561944111961068,81.726772608828,79.967889342274276,78.283055273019713,76.669947211771515,75.125672443384858,73.647102141230988,72.23110671888098,70.874556589905879,69.574322167876772,68.32727386636472,67.129764262412507,65.975460551713596,64.857162113903854,63.767667894405449,62.699776838640545,61.64628789203131,60.599999999999909],[733.33299999999997,722.86585791836922,712.32282381327218,701.62800566124236,690.70551143881346,679.47956710925985,667.95235427498244,656.33869510036118,644.8893329060819,633.85498257357676,623.38725516328384,613.316663075213,603.40880361120344,593.42927420201147,583.22567063086399,572.96220961713459,562.87951790878333,553.21822225377059,544.15897855424384,535.60613633960429,527.3845212886938,519.31895185822805,511.23427390007458,503.01741691088512,494.74959544924144,486.5499261853497,478.53752515386321,470.77919673451817,463.14675096408547,455.47479243552351,447.72683492435721,439.96874361472715,432.26920303972616,424.6968977324471,417.32051222598295,410.2087310534265,403.4302387478707,397.05143233645896,391.07804972860913,385.45033110479631,380.10525963018858,374.97981846995407,370.01099078926097,365.13575975327728,360.29110852717122,355.41468095115448,350.47869313403851,345.50622092826723,340.52441129037254,335.56041117688625,330.64136754434026,325.79442734926641,321.04673754819663,316.42536647965807,311.94632068324137,307.6032349625869,303.38704531264381,299.28868772836131,295.29909820468856,291.40921273657477,287.6099673189691,283.89229794682075,280.24714061507888,276.6654313186927,273.13810605261142,269.65610081178426,266.2103515911603,262.79179438568877,259.39136519031888,255.9999999999998],[1000,715.38000595932851,657.46843965682763,589.93911784152954,526.68240896821646,470.12891447187633,421.33722439961565,380.03398526833217,344.93980311607766,314.75049533923175,288.17972600611745,264.44315565424017,243.315258543021,224.59976002403099,208.09994946708156,193.58811053356405,180.78545222882693,169.4084176184127,159.17361591016268,149.85798883593029,141.38821246250097,133.71357421038306,126.77459818467203,120.50032815673343,114.81903086565586,109.65897305052792,104.94842145043819,100.61564280447527,96.589862001580741,92.824209479775988,89.296807558647032,85.986954108650423,82.873947000242765,79.937084103880608,77.155663290020541,74.50962524794889,71.98981098160229,69.59616065469001,67.328893331200803,65.188228075123448,63.174383950446675,61.287580021159243,59.527312654690711,57.884320964234348,56.343520498883976,54.889721636233013,53.507734753874857,52.182370229402927,50.898438440410629,49.642238821966217,48.413406062398479,47.218603325844086,46.064556883132326,44.957993005092504,43.905637962553918,42.914218026345864,41.988941250758018,41.12474042639554,40.312288470939244,39.542244593917779,38.805268004859762,38.092017913293844,37.393153528748641,36.70044408594719,36.011415155427848,35.325452542832942,34.641942984577589,33.960273217076889,33.279829976745972,32.599999999999945]],"xo":[[0.10000000000000001,0.20000000000000001,0.29999999999999999,1,3,5,7,10,13,15,18,21,24,27,30,33,36,39,41.600000000000001],[2.2999999999999998,4.5999999999999996,6.9000000000000004,9.1999999999999993,11.5,16.100000000000001,18.399999999999999,20.699999999999999],[0.10000000000000001,0.20000000000000001,0.29999999999999999,1,3,5,7,10,14,17,21,24,28,31,35,38,42,45,50],[0.10000000000000001,0.20000000000000001,0.29999999999999999,0.5,0.80000000000000004,1,2,5,10,15,20,25,30,35,40,45,50,55,58.799999999999997],[4,6,8,10,12,14,16],[0.10000000000000001,0.20000000000000001,0.29999999999999999,0.5,0.80000000000000004,1,2,3,4,5,8,18,30,42,54,66,78,89,98.400000000000006],[1.2,2.5,3.7000000000000002,5,6.2000000000000002,7.4000000000000004,8.6999999999999993,9.9000000000000004],[0.10000000000000001,0.20000000000000001,0.29999999999999999,0.40000000000000002,0.59999999999999998,0.80000000000000004,1,2,4,8,12,15,20,25,30,35,40,45,50],[1.5,2.1000000000000001,2.6000000000000001,3.1000000000000001,3.6000000000000001,4.2000000000000002,4.7000000000000002,5,6,7,8,10],[0.10000000000000001,0.20000000000000001,0.40000000000000002,0.5,0.69999999999999996,1,2,4,7,10,13,15,20,25,30,35,40,45,50]],"yo":[[5500,4500,4066.6700000000001,3420,2300,1648,1252.8599999999999,907,706.923,620,522.77800000000002,453.81,397.08300000000003,349.63,316.33300000000003,288.78800000000001,265,246.41,231.49000000000001],[2508.6999999999998,1602.1700000000001,1130.4300000000001,871.73900000000003,708.69600000000003,514.28599999999994,452.71699999999998,404.34800000000001],[3600,3750,3400,2990,1913.3299999999999,1368,1038.5699999999999,756,549.28599999999994,455.88200000000001,372.38099999999997,327.91699999999997,281.42899999999997,253.87100000000001,226.571,207.89500000000001,187.619,175.55600000000001,157.59999999999999],[3800,3450,3300,3040,2775,2660,2040,1168,644,438.66699999999997,331,264.80000000000001,220.333,188,163.75,144.88900000000001,130.19999999999999,117.818,110.20399999999999],[1225,908.33299999999997,712.5,584,491.66699999999997,425,373.75],[4100,2550,2100,2300,1887.5,1830,1415,1170,982.5,840,570,260.55599999999998,154.667,107.857,82.037000000000006,65.757599999999996,54.615400000000001,47.191000000000003,42.479700000000001],[975,832,729.73000000000002,624,545.16099999999994,477.02699999999999,413.79300000000001,368.68700000000001],[1800,1500,1400,1250,1183.3299999999999,1175,1150,965,720,431.25,292.5,232,170.5,133.19999999999999,108.667,91.142899999999997,78,68.222200000000001,60.600000000000001],[733.33299999999997,680.952,634.61500000000001,593.548,552.77800000000002,511.90499999999997,478.72300000000001,460,400,357.14299999999997,317.5,256],[1000,900,750,780,742.85699999999997,700,615,450,300,213,160.76900000000001,136.667,98.5,76,60.666699999999999,50.571399999999997,42.75,37.333300000000001,32.600000000000001]],"z":[{"value":-40,"unit":"\u00b0C","name":"","comment":null,"realZ":-40},{"value":-20,"unit":"\u00b0C","name":"","comment":null,"realZ":-20},{"value":0,"unit":"\u00b0C","name":"","comment":null,"realZ":0},{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23},{"value":40,"unit":"\u00b0C","name":"","comment":null,"realZ":40},{"value":60,"unit":"\u00b0C","name":"","comment":null,"realZ":60},{"value":80,"unit":"\u00b0C","name":"","comment":null,"realZ":80},{"value":90,"unit":"\u00b0C","name":"","comment":null,"realZ":90},{"value":100,"unit":"\u00b0C","name":"","comment":null,"realZ":100},{"value":120,"unit":"\u00b0C","name":"","comment":null,"realZ":120}],"zo":[{"value":-40,"unit":"\u00b0C","name":"","comment":null,"realZ":-40},{"value":-20,"unit":"\u00b0C","name":"","comment":null,"realZ":-20},{"value":0,"unit":"\u00b0C","name":"","comment":null,"realZ":0},{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23},{"value":40,"unit":"\u00b0C","name":"","comment":null,"realZ":40},{"value":60,"unit":"\u00b0C","name":"","comment":null,"realZ":60},{"value":80,"unit":"\u00b0C","name":"","comment":null,"realZ":80},{"value":90,"unit":"\u00b0C","name":"","comment":null,"realZ":90},{"value":100,"unit":"\u00b0C","name":"","comment":null,"realZ":100},{"value":120,"unit":"\u00b0C","name":"","comment":null,"realZ":120}],"keys":["Y - Yield"],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"P","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"secant-modulus-strain-delrin\u00ae-100p-nc010.png","svgname":"secant-modulus-strain-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","Y","","","Y","","Y","","Y",""],"xmarker":[],"option":9},"moist":0,"name":"Secant modulus-strain","shortname":"Es &#949;"},{"id":33,"addId":[],"data":{"name":"Creep curve 90 \u00b0C","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Time in","unit":"h","log":true},"y":{"name":"Strain in","unit":"%","log":false},"z":{"name":"","unit":"MPa"}},"x":[[0.0030000000000000009,0.0035138555237121741,0.0041157268805075177,0.00482068987772067,0.0056464025849773782,0.0066135476374418172,0.0077463502990528389,0.0090731852623120862,0.01062728738387974,0.012447584158640843,0.01457967078423743,0.017076952239699232,0.020001980985212046,0.023428023790024413,0.027440896934745839,0.032141115756591045,0.037646412379856616,0.044094684696301858,0.05164745046214899,0.06049389303069104,0.07085560005891571,0.082992113884320554,0.097207432598989868,0.11385762466127979,0.13335974777759513,0.15620229545638831,0.18295743290198366,0.21429532873561155,0.25100094152778157,0.2939936816147839,0.34435044069286214,0.40333256604044498,0.47241745502474086,0.55333556127891104,0.64811373948875917,0.75912601449877637,0.88915304641337778,1.0414517811883848,1.2198370313362292,1.4287770301964899,1.6735053532363371,1.9601520098104652,2.2958969889960072,2.689150105552589,3.1497616508290469,3.6892691250474736,4.3211862311696141,5.0613413691281126,5.9282741091012516,6.9436995747817658,8.1330523686149263,9.5261236633659792,11.157807418027931,13.068974409451373,15.307495972634587,17.92944309254797,21.000490882610926,24.597563629509853,28.81076160980496,33.745617941655937,39.52574200178946,46.295915620603402,54.225719609590001,63.513781459141804,74.392750604017778,87.135125878023345,102.06008112528261,119.54145993752893,140.01713977136779,164],[0.0023000000000000008,0.0026203043291124798,0.0029852151205067828,0.0034009443928678059,0.0038745692676966617,0.0044141524459094476,0.0050288794623386795,0.0057292150546742939,0.0065270813087736695,0.007436060612977735,0.0084716268764036314,0.0096514089473330698,0.010995490715970328,0.01252675301033614,0.014271263105524592,0.016258718477090994,0.018522952352757645,0.021102509668641318,0.024041303234729906,0.027389361279768962,0.031203679101306222,0.035549189318864902,0.040499867247243825,0.046139990207145078,0.052565572210865059,0.059885998446262752,0.068225887383463246,0.077727212203664867,0.088551717663959709,0.10088367354139985,0.11493301152926093,0.13093889898611169,0.14917381037501309,0.1699481657025439,0.19361561491960902,0.2205790582424462,0.25129750488010244,0.2862938869271725,0.326163961440743,0.37158645224506726,0.42333460411186841,0.48228934600758538,0.54945428749065328,0.62597280354833551,0.71314749871494743,0.81246238181674491,0.92560812883280552,1.0545108639314356,1.201364948632905,1.3686703372812141,1.5592751347416534,1.7764240808004343,2.0238137866352326,2.3056556636686172,2.6267476160667762,2.9925557173328947,3.4093072614076889,3.8840967723222519,4.425006777046872,5.0412453974991207,5.7433031039936129,6.5431312986085235,7.4543457685631624,8.4924584730727606,9.6751416094784837,11.02252845395337,12.557556098112823,14.306355916068625,16.298698408999364,18.568499999999872],[0.0049999999999999992,0.0054234633460488752,0.0058827909331871341,0.0063810201997218166,0.0069214458327177507,0.0075076415550814927,0.0081434837578515731,0.008833177133970473,0.0095812824830491857,0.010392746870991478,0.011272936343917281,0.012227671412715515,0.013263265542878449,0.014386566904142856,0.015605003656019719,0.016926633068676322,0.018360194803996959,0.019915168709158899,0.021601837504900547,0.023431354783026395,0.025415818762802123,0.027568352293975709,0.029903189635467925,0.032435770583581776,0.035182842572181204,0.038162571420006529,0.041394661457475543,0.044900485827344135,0.048703227820877562,0.052828034184159448,0.057302181408321134,0.062155256103334576,0.067419350648143125,0.073129275410924122,0.079322788942852024,0.086040847667585768,0.093327876717625227,0.10123206370852171,0.10980567739361041,0.11910541330646272,0.1291927686767205,0.14013444909855297,0.15200280964095078,0.16487633331682822,0.17884015007495094,0.19398659974667529,0.21041584267014946,0.22823652202990849,0.24756648229177705,0.26853354848394212,0.29127637147741975,0.31594534485558035,0.34270359943580225,0.37172808201981788,0.40321072550630632,0.43735971810344526,0.47440088003446074,0.5145791568400454,0.5581602391525442,0.60543231965313948,0.65670799883042952,0.71232635214278828,0.77265517225422298,0.83809340117117148,0.90907376836345666,0.98606565231474641,1.06957818442536,1.1601636157928887,1.2584209691344521,1.365]],"y":[[0.48999999999999999,0.63672966582173673,0.73081402005619356,0.75662635410876378,0.77818893532442335,0.80963312663386389,0.83525416473658043,0.86152421709027061,0.8903822903356392,0.91638628143196166,0.94935698970075599,0.98141166624314402,1.0100207545851034,1.0449078484805596,1.0760275033431346,1.1111302843948765,1.1489328275033601,1.1807505782048429,1.2171957909404849,1.251908168162567,1.293552383634994,1.3403345089806882,1.3745238093393324,1.4131494263378621,1.4660185171220965,1.5037483164580883,1.5550863526405354,1.6012860250969538,1.6511052062005782,1.6933131804016091,1.7541030478531268,1.8025329981210638,1.8580928997600712,1.9208535683000467,1.9833793380657594,2.039484101328533,2.1044366491411663,2.1769748393173574,2.246103188690332,2.3196554558196874,2.3932511296143169,2.46250723365119,2.5403500899433626,2.6187277118509216,2.6924394729062966,2.7699927890029898,2.8428249715649687,2.9322947835962827,3.0523951334849149,3.1549502576039479,3.2499964558345233,3.3416932003283537,3.4305104331326333,3.5225896480920675,3.6123867968413639,3.7079651896635357,3.8000106782902074,3.9024095339561735,4.006998639056178,4.104912316658555,4.2105099652399396,4.3411858010024567,4.4515293504208149,4.5549452207447905,4.6729690117913529,4.8012279709285695,4.9104317711258485,5.017758635863875,5.1300726992223407,5.2400000000000002],[1.96,2.041399157407918,2.107643869246127,2.1745718252939104,2.2278300574687435,2.2818400047076,2.3386402587525743,2.3914428677678243,2.4436362209669422,2.4959226659312179,2.5489262340481722,2.6037176610102644,2.6561140669373651,2.7108716896030285,2.7656780936113616,2.8224832568213065,2.8815613068301049,2.9500486785729469,2.9989269800197085,3.0688899363137536,3.1265250742693524,3.1940227547886115,3.2693635762608797,3.3311504376595247,3.4059848849753718,3.488524899424982,3.551015284072133,3.6385328623913993,3.719050247978132,3.795573521179334,3.8957061200537999,3.9704624315420567,4.0753409718312241,4.1549811792163576,4.2696137866007735,4.3590087430679558,4.4723559994951021,4.5835466065735169,4.6932151403131108,4.8297373572165716,4.9500932312035326,5.0844970736059985,5.2384624893991099,5.3850303493858442,5.5388363963332043,5.7100427616613576,5.8878322576157238,6.0830217921800438,6.3003743544170971,6.5343976045714349,6.7686056367816221,7.010851647443797,7.3055212853916851,7.5983942717140476,7.93955239740158,8.2907895955472526,8.6938784414820134,9.1266450505876904,9.6061541229009215,10.163762880286852,10.775958519779566,11.491519468420282,12.485709980621181,13.703528375823623,15.250492455893678,17.237125073504593,20.050202912122288,24.351132004964295,31.924344101216509,49.99999999999531],[2.4300000000000002,2.6102672205274247,2.7264947289039383,2.824494997260016,2.8859215863134065,2.9864755132470071,3.03371686250712,3.1045734526824496,3.1815843730722748,3.2269144053657479,3.3070252166905543,3.3765875285813829,3.4250351238446193,3.4991921291631787,3.5560872970948472,3.6284779777635072,3.7026398407204537,3.7615219336121393,3.8347377131704801,3.9146937588900319,3.9911777980668983,4.0563627090118581,4.129584282703366,4.2267915367726143,4.2901814700198928,4.3965653332024948,4.4553599564152426,4.5775976826565952,4.6475950087144264,4.7695464422201654,4.8479856111762309,4.9740812364233316,5.0715477908516977,5.1949604384140917,5.3139868945006841,5.4348232487263219,5.57334392814899,5.7184732387287971,5.855128203606105,5.9983423813918026,6.1719768467617691,6.3488276705909428,6.5255275670422037,6.7206240928656289,6.9283576384329679,7.1391489370962438,7.3650678463278743,7.6224965113618781,7.8925165382594686,8.1885937528329418,8.515233229647011,8.8648220771620121,9.2481741222065317,9.675072654700875,10.131321276727951,10.662563420893282,11.255763146865913,11.909403751738868,12.689847368731447,13.578975962884188,14.588554376220257,15.768611052816274,17.168042584240833,18.832552636159075,20.909550920260944,23.578887518365448,27.087654485163021,31.902360900659577,38.919279476646793,50.000000000000099]],"xo":[[0.0030000000000000001,0.0040000000000000001,0.0050000000000000001,0.0060000000000000001,0.0070000000000000001,0.0080000000000000002,0.0089999999999999993,0.01,0.012,0.014,0.016,0.017999999999999999,0.02,0.024,0.028000000000000001,0.032000000000000001,0.035999999999999997,0.040000000000000001,0.050000000000000003,0.059999999999999998,0.070000000000000007,0.080000000000000002,0.089999999999999997,0.10000000000000001,0.12,0.14000000000000001,0.16,0.17999999999999999,0.20000000000000001,0.25,0.29999999999999999,0.34999999999999998,0.40000000000000002,0.45000000000000001,0.5,0.57999999999999996,0.66000000000000003,0.73999999999999999,0.81999999999999995,0.90000000000000002,1,1.1000000000000001,1.2,1.3,1.3999999999999999,1.5,1.6000000000000001,1.7,1.8,1.8999999999999999,2,2.2000000000000002,2.3999999999999999,2.6000000000000001,2.7999999999999998,3,3.2000000000000002,3.3999999999999999,3.6000000000000001,3.7999999999999998,4,4.2000000000000002,4.4000000000000004,4.5999999999999996,4.7999999999999998,5,5.2000000000000002,5.4000000000000004,5.5999999999999996,5.7999999999999998,6,6.25,6.5,6.75,7,7.5,8,8.5,9,9.5,10,10.5,11,11.5,12,12.5,13,13.5,14,14.5,15,15.5,16,16.5,17,17.5,18,18.5,19,19.5,20,20.5,21,21.5,22,22.5,23,23.5,24,24.5,25,25.5,26,26.5,27,27.5,28,28.5,29,29.5,30,30.5,31,31.5,32,32.5,33,33.5,34,34.5,35,35.5,36,36.5,37,37.5,38.5,39,39.5,40,40.5,41,43,43.5,44,44.5,45,45.5,46,47,47.5,48,50,51,51.5,52,52.5,53,54,55,55.5,56,57,58,58.5,60,62,64,65,65.5,66,66.5,67,70,71,72,74,75,75.5,76,80,81,82,83,84,85,87,88,90,91,92,94,96,98,100,102,104,106,108,110,112,114,116,118,120,122,124,126,128,130,134,136,138,140,142,144,146,150,152,154,156,160,162,164],[0.0023,0.0025000000000000001,0.0027000000000000001,0.0030000000000000001,0.0033,0.0037000000000000002,0.0041999999999999997,0.0047000000000000002,0.0053,0.0060000000000000001,0.0067999999999999996,0.0077000000000000002,0.0086999999999999994,0.0097999999999999997,0.0111,0.012500000000000001,0.0141,0.015699999999999999,0.017500000000000002,0.019099999999999999,0.021100000000000001,0.0241,0.026499999999999999,0.029100000000000001,0.033000000000000002,0.035900000000000001,0.039199999999999999,0.042799999999999998,0.048099999999999997,0.0521,0.0562,0.061199999999999997,0.068099999999999994,0.073599999999999999,0.079000000000000001,0.085300000000000001,0.094200000000000006,0.10150000000000001,0.1084,0.1157,0.1275,0.1356,0.14480000000000001,0.154,0.16889999999999999,0.17829999999999999,0.18959999999999999,0.20030000000000001,0.21809999999999999,0.2301,0.24279999999999999,0.26219999999999999,0.27650000000000002,0.29110000000000003,0.30630000000000002,0.32890000000000003,0.34539999999999998,0.3624,0.37859999999999999,0.40450000000000003,0.42330000000000001,0.4425,0.46139999999999998,0.49099999999999999,0.51149999999999995,0.53269999999999995,0.5554,0.58779999999999999,0.60950000000000004,0.63319999999999999,0.65790000000000004,0.69289999999999996,0.71830000000000005,0.7429,0.78169999999999995,0.80710000000000004,0.83520000000000005,0.8629,0.9042,0.93210000000000004,0.9607,0.99129999999999996,1.0333000000000001,1.0648,1.0963000000000001,1.1278999999999999,1.1694,1.2011000000000001,1.2378,1.2644,1.3161,1.3478000000000001,1.3794,1.4278,1.4794,1.5111000000000001,1.5478000000000001,1.5793999999999999,1.6311,1.6677999999999999,1.7161,1.7678,1.8044,1.8411,1.8894,1.9460999999999999,1.9827999999999999,2.0194000000000001,2.0678000000000001,2.1294,2.1610999999999998,2.2143999999999999,2.2561,2.3077999999999999,2.3660999999999999,2.3978000000000002,2.4344000000000001,2.5127999999999999,2.5493999999999999,2.5861000000000001,2.6394000000000002,2.7010999999999998,2.7544,2.7911000000000001,2.8328000000000002,2.9060999999999999,2.9478,3.0061,3.0678000000000001,3.1044,3.1627999999999998,3.2044000000000001,3.2827999999999999,3.3193999999999999,3.3778000000000001,3.4144000000000001,3.4977999999999998,3.5344000000000002,3.5760999999999998,3.6343999999999999,3.6960999999999999,3.7544,3.7961,3.8494000000000002,3.9161000000000001,3.9744000000000002,4.0160999999999998,4.0743999999999998,4.1360999999999999,4.1943999999999999,4.2361000000000004,4.3193999999999999,4.3611000000000004,4.4194000000000004,4.4611000000000001,4.5278,4.5861000000000001,4.6277999999999997,4.6860999999999997,4.7527999999999997,4.8110999999999997,4.8528000000000002,4.9577999999999998,5.0827999999999998,5.1828000000000003,5.3128000000000002,5.4127999999999998,5.5427999999999997,5.6428000000000003,5.7728000000000002,5.8777999999999997,6.0077999999999996,6.0911,6.2210999999999999,6.3261000000000003,6.4561000000000002,6.5510999999999999,6.6494,6.7393999999999998,6.8444000000000003,6.9344000000000001,7.0178000000000003,7.1028000000000002,7.2077999999999998,7.2760999999999996,7.3811,7.4661,7.5544000000000002,7.6394000000000002,7.7278000000000002,7.8277999999999999,7.8960999999999997,8.0010999999999992,8.0693999999999999,8.1693999999999996,8.2378,8.3377999999999997,8.4061000000000003,8.4893999999999998,8.5744000000000007,8.6577999999999999,8.7210999999999999,8.8210999999999995,8.8894000000000002,8.9678000000000004,9.0360999999999994,9.1361000000000008,9.1994000000000007,9.2777999999999992,9.3411000000000008,9.4244000000000003,9.5076000000000001,9.5907,9.6402999999999999,9.7236999999999991,9.8059999999999992,9.8887999999999998,9.9720999999999993,10.0037,10.085599999999999,10.1678,10.2003,10.2813,10.363,10.394500000000001,10.475,10.555300000000001,10.636900000000001,10.667400000000001,10.746,10.8256,10.8546,10.933,11.0121,11.041,11.1195,11.1472,11.2257,11.3024,11.379200000000001,11.4061,11.4823,11.5085,11.584899999999999,11.661099999999999,11.686500000000001,11.7623,11.7883,11.863200000000001,11.937900000000001,11.9625,12.0367,12.059900000000001,12.133900000000001,12.1579,12.230399999999999,12.305,12.328200000000001,12.400700000000001,12.423999999999999,12.4969,12.518599999999999,12.591100000000001,12.613,12.6844,12.706099999999999,12.7775,12.798500000000001,12.8698,12.8912,12.9618,12.982100000000001,13.053100000000001,13.073,13.142899999999999,13.1631,13.2326,13.252000000000001,13.271699999999999,13.3408,13.3599,13.4292,13.448399999999999,13.5167,13.535399999999999,13.603899999999999,13.622299999999999,13.6907,13.7088,13.7262,13.794,13.8118,13.829000000000001,13.8962,13.913399999999999,13.9801,13.997400000000001,14.0642,14.080500000000001,14.097300000000001,14.1638,14.1799,14.2464,14.262499999999999,14.278,14.344200000000001,14.3597,14.3748,14.4404,14.455399999999999,14.4703,14.535600000000001,14.5503,14.5649,14.6296,14.6442,14.708600000000001,14.7232,14.7372,14.801,14.8154,14.828799999999999,14.8927,14.9068,14.920299999999999,14.983599999999999,14.997299999999999,15.0105,15.0238,15.087400000000001,15.100199999999999,15.113,15.1761,15.188700000000001,15.201499999999999,15.2645,15.2767,15.289400000000001,15.3017,15.3637,15.375999999999999,15.388,15.4498,15.4618,15.473599999999999,15.4849,15.546799999999999,15.5581,15.5694,15.631,15.642099999999999,15.6531,15.6646,15.7255,15.7363,15.747400000000001,15.7578,15.8188,15.829499999999999,15.84,15.8507,15.911,15.9213,15.931699999999999,15.9419,16.001999999999999,16.0122,16.022099999999998,16.0319,16.042000000000002,16.101700000000001,16.1114,16.121300000000002,16.130700000000001,16.190300000000001,16.1998,16.209299999999999,16.218699999999998,16.277999999999999,16.287099999999999,16.296399999999998,16.305499999999999,16.314399999999999,16.3736,16.3826,16.391500000000001,16.400500000000001,16.459199999999999,16.468,16.477,16.485399999999998,16.4941,16.552700000000002,16.561,16.569500000000001,16.577999999999999,16.586099999999998,16.644600000000001,16.652799999999999,16.661000000000001,16.6692,16.677099999999999,16.735199999999999,16.743400000000001,16.751100000000001,16.7591,16.767099999999999,16.774699999999999,16.832599999999999,16.840299999999999,16.847799999999999,16.855499999999999,16.863,16.9207,16.9284,16.935400000000001,16.943000000000001,16.950299999999999,16.9574,17.014700000000001,17.021999999999998,17.0291,17.036300000000001,17.043099999999999,17.0504,17.107500000000002,17.1143,17.121600000000001,17.128399999999999,17.135100000000001,17.142199999999999,17.198899999999998,17.2057,17.212499999999999,17.218900000000001,17.2257,17.232399999999998,17.288799999999998,17.295300000000001,17.3017,17.3081,17.314599999999999,17.320799999999998,17.327300000000001,17.383400000000002,17.389500000000002,17.396100000000001,17.402000000000001,17.408200000000001,17.414400000000001,17.420400000000001,17.476600000000001,17.482600000000001,17.488299999999999,17.494499999999999,17.5002,17.5061,17.512,17.567499999999999,17.573499999999999,17.5793,17.584800000000001,17.590800000000002,17.5961,17.601900000000001,17.657499999999999,17.6629,17.668500000000002,17.673999999999999,17.679400000000001,17.684999999999999,17.690200000000001,17.695699999999999,17.751000000000001,17.7562,17.761700000000001,17.7669,17.771899999999999,17.7774,17.782399999999999,17.787600000000001,17.8428,17.8477,17.852900000000002,17.857900000000001,17.8629,17.867899999999999,17.872699999999998,17.877700000000001,17.932700000000001,17.9375,17.942399999999999,17.947199999999999,17.951899999999998,17.956700000000001,17.961300000000001,17.966100000000001,17.970800000000001,18.025400000000001,18.030100000000001,18.034700000000001,18.039100000000001,18.043700000000001,18.048200000000001,18.052700000000002,18.057200000000002,18.061599999999999,18.116,18.1204,18.124700000000001,18.129100000000001,18.133400000000002,18.137699999999999,18.141999999999999,18.1462,18.150400000000001,18.204599999999999,18.2087,18.212800000000001,18.216899999999999,18.221,18.225100000000001,18.228999999999999,18.233000000000001,18.236999999999998,18.241,18.294899999999998,18.2988,18.302700000000002,18.3065,18.310300000000002,18.3142,18.317900000000002,18.3217,18.325299999999999,18.3291,18.332899999999999,18.386399999999998,18.3902,18.393799999999999,18.397300000000001,18.4011,18.404499999999999,18.408100000000001,18.4117,18.415099999999999,18.418700000000001,18.4221,18.4756,18.479099999999999,18.482500000000002,18.485900000000001,18.4893,18.4925,18.495999999999999,18.499199999999998,18.502600000000001,18.5059,18.5092,18.5626,18.565799999999999,18.5685],[0.0050000000000000001,0.0051000000000000004,0.0051999999999999998,0.0054000000000000003,0.0054999999999999997,0.0057000000000000002,0.0060000000000000001,0.0061999999999999998,0.0067000000000000002,0.0070000000000000001,0.0073000000000000001,0.0076,0.0083999999999999995,0.0088000000000000005,0.0091999999999999998,0.0099000000000000008,0.010699999999999999,0.0112,0.0118,0.012699999999999999,0.0137,0.0144,0.0155,0.016299999999999999,0.017399999999999999,0.0183,0.019699999999999999,0.0206,0.021999999999999999,0.023,0.0246,0.025600000000000001,0.027300000000000001,0.029100000000000001,0.0304,0.031600000000000003,0.033399999999999999,0.035499999999999997,0.036799999999999999,0.038300000000000001,0.041200000000000001,0.042700000000000002,0.0441,0.045699999999999998,0.048800000000000003,0.0504,0.052200000000000003,0.053900000000000003,0.0574,0.059200000000000003,0.060999999999999999,0.063700000000000007,0.066500000000000004,0.068500000000000005,0.070400000000000004,0.073499999999999996,0.076399999999999996,0.0785,0.081600000000000006,0.083699999999999997,0.086900000000000005,0.088999999999999996,0.092299999999999993,0.094500000000000001,0.097900000000000001,0.1002,0.1037,0.1072,0.1095,0.11310000000000001,0.1154,0.1192,0.1216,0.12529999999999999,0.1278,0.13159999999999999,0.1353,0.13780000000000001,0.14019999999999999,0.14419999999999999,0.14810000000000001,0.1507,0.15340000000000001,0.15740000000000001,0.1613,0.16389999999999999,0.16650000000000001,0.1719,0.17460000000000001,0.1774,0.18010000000000001,0.18559999999999999,0.1883,0.191,0.19500000000000001,0.19919999999999999,0.20200000000000001,0.20480000000000001,0.2089,0.2132,0.21590000000000001,0.21870000000000001,0.2228,0.22700000000000001,0.2298,0.2339,0.23669999999999999,0.24110000000000001,0.24390000000000001,0.24809999999999999,0.25090000000000001,0.25519999999999998,0.25929999999999997,0.2621,0.26640000000000003,0.26919999999999999,0.2732,0.2762,0.28039999999999998,0.2833,0.2873,0.29020000000000001,0.29449999999999998,0.2984,0.30130000000000001,0.30409999999999998,0.30840000000000001,0.3125,0.31519999999999998,0.318,0.3236,0.32640000000000002,0.32919999999999999,0.33189999999999997,0.33739999999999998,0.34010000000000001,0.34279999999999999,0.34560000000000002,0.35099999999999998,0.35370000000000001,0.35639999999999999,0.3604,0.36470000000000002,0.36730000000000002,0.37,0.37390000000000001,0.37809999999999999,0.38080000000000003,0.3846,0.38729999999999998,0.39140000000000003,0.39410000000000001,0.39800000000000002,0.40050000000000002,0.4047,0.4073,0.41099999999999998,0.41370000000000001,0.41760000000000003,0.42130000000000001,0.4239,0.42780000000000001,0.43049999999999999,0.43409999999999999,0.43659999999999999,0.44059999999999999,0.44429999999999997,0.44679999999999997,0.44929999999999998,0.45319999999999999,0.45679999999999998,0.4592,0.4617,0.46539999999999998,0.46899999999999997,0.47160000000000002,0.47399999999999998,0.47889999999999999,0.48120000000000002,0.48359999999999997,0.48599999999999999,0.49070000000000003,0.49309999999999998,0.49540000000000001,0.49880000000000002,0.50249999999999995,0.50480000000000003,0.50700000000000001,0.51049999999999995,0.5141,0.51639999999999997,0.51870000000000005,0.52200000000000002,0.52549999999999997,0.52769999999999995,0.53090000000000004,0.53320000000000001,0.53669999999999995,0.53900000000000003,0.5423,0.5444,0.54800000000000004,0.55110000000000003,0.55330000000000001,0.55559999999999998,0.55889999999999995,0.56200000000000006,0.56420000000000003,0.56630000000000003,0.56969999999999998,0.57269999999999999,0.57489999999999997,0.57820000000000005,0.58130000000000004,0.58350000000000002,0.58560000000000001,0.58889999999999998,0.59189999999999998,0.59399999999999997,0.59599999999999997,0.60019999999999996,0.60229999999999995,0.60429999999999995,0.60640000000000005,0.61050000000000004,0.61260000000000003,0.61460000000000004,0.61660000000000004,0.62070000000000003,0.62270000000000003,0.62480000000000002,0.62770000000000004,0.63080000000000003,0.63280000000000003,0.63480000000000003,0.63759999999999994,0.64070000000000005,0.64259999999999995,0.64549999999999996,0.64749999999999996,0.65049999999999997,0.65249999999999997,0.6552,0.65720000000000001,0.66020000000000001,0.66210000000000002,0.66500000000000004,0.66690000000000005,0.66979999999999995,0.67259999999999998,0.6744,0.67620000000000002,0.67920000000000003,0.68179999999999996,0.68369999999999997,0.68559999999999999,0.68920000000000003,0.69110000000000005,0.69299999999999995,0.69589999999999996,0.69850000000000001,0.70030000000000003,0.70220000000000005,0.70499999999999996,0.70760000000000001,0.70940000000000003,0.71120000000000005,0.71460000000000001,0.71650000000000003,0.71819999999999995,0.71989999999999998,0.72350000000000003,0.72519999999999996,0.72709999999999997,0.72960000000000003,0.73229999999999995,0.73409999999999997,0.73580000000000001,0.73829999999999996,0.74099999999999999,0.74260000000000004,0.74429999999999996,0.74680000000000002,0.74939999999999996,0.75109999999999999,0.75349999999999995,0.75519999999999998,0.75790000000000002,0.75949999999999995,0.76190000000000002,0.76370000000000005,0.76619999999999999,0.76859999999999995,0.77029999999999998,0.77190000000000003,0.77439999999999998,0.77669999999999995,0.77829999999999999,0.78000000000000003,0.78239999999999998,0.78469999999999995,0.78639999999999999,0.78790000000000004,0.79120000000000001,0.79279999999999995,0.79430000000000001,0.79590000000000005,0.79910000000000003,0.80059999999999998,0.80220000000000002,0.80520000000000003,0.80679999999999996,0.80840000000000001,0.80989999999999995,0.81289999999999996,0.81440000000000001,0.81589999999999996,0.81740000000000002,0.82040000000000002,0.82189999999999996,0.82350000000000001,0.8256,0.82789999999999997,0.82940000000000003,0.83089999999999997,0.83299999999999996,0.83530000000000004,0.8367,0.83879999999999999,0.84030000000000005,0.84250000000000003,0.84389999999999998,0.84599999999999997,0.84740000000000004,0.84960000000000002,0.85099999999999998,0.85299999999999998,0.85450000000000004,0.85660000000000003,0.85860000000000003,0.86009999999999998,0.86140000000000005,0.86360000000000003,0.86560000000000004,0.86699999999999999,0.86829999999999996,0.87109999999999999,0.87239999999999995,0.87380000000000002,0.87519999999999998,0.87780000000000002,0.87919999999999998,0.88049999999999995,0.88180000000000003,0.88439999999999996,0.88570000000000004,0.88700000000000001,0.88900000000000001,0.89100000000000001,0.89229999999999998,0.89359999999999995,0.89549999999999996,0.89749999999999996,0.89880000000000004,0.90059999999999996,0.90259999999999996,0.90390000000000004,0.90510000000000002,0.90700000000000003,0.90880000000000005,0.91010000000000002,0.9113,0.91310000000000002,0.91500000000000004,0.91620000000000001,0.91800000000000004,0.91920000000000002,0.92120000000000002,0.9224,0.92420000000000002,0.9254,0.92730000000000001,0.92900000000000005,0.93020000000000003,0.93140000000000001,0.93320000000000003,0.93489999999999995,0.93610000000000004,0.93720000000000003,0.93899999999999995,0.94069999999999998,0.94189999999999996,0.94299999999999995,0.94530000000000003,0.94650000000000001,0.94769999999999999,0.94879999999999998,0.95109999999999995,0.95220000000000005,0.95340000000000003,0.95509999999999995,0.95679999999999998,0.95789999999999997,0.95899999999999996,0.96060000000000001,0.96230000000000004,0.96340000000000003,0.96450000000000002,0.96609999999999996,0.96779999999999999,0.96889999999999998,0.97050000000000003,0.97160000000000002,0.97319999999999995,0.97430000000000005,0.97589999999999999,0.97699999999999998,0.97860000000000003,0.97970000000000002,0.98129999999999995,0.9829,0.98399999999999999,0.98550000000000004,0.98650000000000004,0.98819999999999997,0.98919999999999997,0.99070000000000003,0.99170000000000003,0.99329999999999996,0.99480000000000002,0.99580000000000002,0.99680000000000002,0.99839999999999995,0.99990000000000001,1.0008999999999999,1.0019,1.0035000000000001,1.0048999999999999,1.0059,1.0068999999999999,1.0088999999999999,1.0099,1.0108999999999999,1.0118,1.0138,1.0147999999999999,1.0158,1.0172000000000001,1.0186999999999999,1.0196000000000001,1.0206,1.022,1.0235000000000001,1.0244,1.0254000000000001,1.0266999999999999,1.0282,1.0290999999999999,1.0305,1.0315000000000001,1.0328999999999999,1.0338000000000001,1.0351999999999999,1.0361,1.0376000000000001,1.0388999999999999,1.0398000000000001,1.0407999999999999,1.0422,1.0435000000000001,1.0444,1.0452999999999999,1.0467,1.048,1.0488999999999999,1.0498000000000001,1.0516000000000001,1.0524,1.0532999999999999,1.0547,1.056,1.0569,1.0578000000000001,1.0590999999999999,1.0604,1.0612999999999999,1.0622,1.0639000000000001,1.0648,1.0656000000000001,1.0664,1.0682,1.069,1.0698000000000001,1.0710999999999999,1.0723,1.0731999999999999,1.0740000000000001,1.0751999999999999,1.0765,1.0773999999999999,1.0782,1.0793999999999999,1.0807,1.0814999999999999,1.0827,1.0835999999999999,1.0848,1.0857000000000001,1.0868,1.0875999999999999,1.0889,1.0900000000000001,1.0908,1.0916999999999999,1.0929,1.0940000000000001,1.0948,1.0955999999999999,1.0968,1.0979000000000001,1.0987,1.0994999999999999,1.101,1.1017999999999999,1.1026,1.1033999999999999,1.1049,1.1056999999999999,1.1065,1.1072,1.1088,1.1094999999999999,1.1103000000000001,1.1113999999999999,1.1125,1.1133,1.1140000000000001,1.1151,1.1162000000000001,1.117,1.1180000000000001,1.1192,1.1198999999999999,1.1206,1.1216999999999999,1.1228,1.1235999999999999,1.1243000000000001,1.1254,1.1265000000000001,1.1272,1.1283000000000001,1.129,1.1301000000000001,1.1308,1.1317999999999999,1.1325000000000001,1.1335999999999999,1.1343000000000001,1.1354,1.1361000000000001,1.1372,1.1382000000000001,1.1389,1.1395,1.1406000000000001,1.1415999999999999,1.1423000000000001,1.143,1.1443000000000001,1.145,1.1456999999999999,1.1464000000000001,1.1477999999999999,1.1484000000000001,1.1491,1.1497999999999999,1.1511,1.1517999999999999,1.1525000000000001,1.1535,1.1545000000000001,1.1552,1.1557999999999999,1.1568000000000001,1.1577999999999999,1.1585000000000001,1.1591,1.1600999999999999,1.1611,1.1617,1.1627000000000001,1.1633,1.1642999999999999,1.1649,1.1657999999999999,1.1665000000000001,1.1675,1.1684000000000001,1.169,1.1697,1.1707000000000001,1.1716,1.1721999999999999,1.1729000000000001,1.1738,1.1748000000000001,1.1754,1.1759999999999999,1.1773,1.1778999999999999,1.1785000000000001,1.1795,1.1802999999999999,1.1809000000000001,1.1816,1.1825000000000001,1.1834,1.1839999999999999,1.1846000000000001,1.1858,1.1863999999999999,1.1870000000000001,1.1876,1.1888000000000001,1.1894,1.1899999999999999,1.1908000000000001,1.1917,1.1923999999999999,1.1930000000000001,1.1938,1.1947000000000001,1.1953,1.1959,1.1968000000000001,1.1977,1.1981999999999999,1.1991000000000001,1.1997,1.2004999999999999,1.2011000000000001,1.2019,1.2024999999999999,1.2034,1.2039,1.2047000000000001,1.2053,1.2061999999999999,1.2070000000000001,1.2076,1.2081,1.2090000000000001,1.2098,1.2103999999999999,1.2109000000000001,1.2121,1.2125999999999999,1.2131000000000001,1.2137,1.2148000000000001,1.2153,1.2159,1.2164999999999999,1.2175,1.2181,1.2185999999999999,1.2194,1.2202,1.2208000000000001,1.2213000000000001,1.2221,1.2229000000000001,1.2234,1.224,1.2246999999999999,1.2255,1.2261,1.2267999999999999,1.2273000000000001,1.2282,1.2286999999999999,1.2294,1.23,1.2307999999999999,1.2315,1.2321,1.2325999999999999,1.2334000000000001,1.2341,1.2346999999999999,1.2354000000000001,1.236,1.2366999999999999,1.2372000000000001,1.238,1.2386999999999999,1.2392000000000001,1.2397,1.2404999999999999,1.2412000000000001,1.2417,1.2422,1.2430000000000001,1.2437,1.2442,1.2446999999999999,1.2457,1.2462,1.2466999999999999,1.2471000000000001,1.2481,1.2485999999999999,1.2491000000000001,1.2496,1.2505999999999999,1.2511000000000001,1.2515000000000001,1.2523,1.2529999999999999,1.2535000000000001,1.254,1.2546999999999999,1.2554000000000001,1.2559,1.2565999999999999,1.2569999999999999,1.2578,1.2582,1.2588999999999999,1.2594000000000001,1.2601,1.2605999999999999,1.2613000000000001,1.2617,1.2624,1.2630999999999999,1.2636000000000001,1.264,1.2646999999999999,1.2654000000000001,1.2659,1.2663,1.2669999999999999,1.2677,1.2681,1.2685999999999999,1.2695000000000001,1.27,1.2704,1.2708999999999999,1.2718,1.2722,1.2726999999999999,1.2733000000000001,1.274,1.2745,1.2748999999999999,1.2755000000000001,1.2762,1.2766999999999999,1.2770999999999999,1.2777000000000001,1.2784,1.2787999999999999,1.2795000000000001,1.2799,1.2806,1.2809999999999999,1.2816000000000001,1.2821,1.2827,1.2831999999999999,1.2838000000000001,1.2842,1.2848999999999999,1.2855000000000001,1.2859,1.2864,1.2869999999999999,1.2876000000000001,1.2881,1.2885,1.2891999999999999,1.2898000000000001,1.2902,1.2906,1.2915000000000001,1.2919,1.2923,1.2927,1.2935000000000001,1.2939000000000001,1.2944,1.2948999999999999,1.2956000000000001,1.296,1.2964,1.2969999999999999,1.2976000000000001,1.298,1.2984,1.2989999999999999,1.2996000000000001,1.3,1.3006,1.3009999999999999,1.3017000000000001,1.3021,1.3026,1.3029999999999999,1.3036000000000001,1.304,1.3046,1.3049999999999999,1.3056000000000001,1.3062,1.3066,1.3069999999999999,1.3076000000000001,1.3082,1.3086,1.3089999999999999,1.3096000000000001,1.3101,1.3105,1.3110999999999999,1.3117000000000001,1.3120000000000001,1.3125,1.3129999999999999,1.3136000000000001,1.3140000000000001,1.3143,1.3147,1.3154999999999999,1.3159000000000001,1.3163,1.3168,1.3173999999999999,1.3178000000000001,1.3181,1.3187,1.3192999999999999,1.3196000000000001,1.3200000000000001,1.3206,1.3210999999999999,1.3214999999999999,1.3220000000000001,1.3224,1.323,1.3233999999999999,1.3239000000000001,1.3243,1.3248,1.3251999999999999,1.3257000000000001,1.3261000000000001,1.3267,1.3271999999999999,1.3275999999999999,1.3279000000000001,1.3285,1.329,1.3292999999999999,1.3299000000000001,1.3304,1.3308,1.3310999999999999,1.3317000000000001,1.3322000000000001,1.3325,1.3329,1.3333999999999999,1.3340000000000001,1.3343,1.3347,1.3353999999999999,1.3357000000000001,1.3360000000000001,1.3364,1.3371,1.3373999999999999,1.3378000000000001,1.3382000000000001,1.3389,1.3391999999999999,1.3395999999999999,1.3401000000000001,1.3406,1.3409,1.3412999999999999,1.3418000000000001,1.3423,1.3426,1.343,1.3434999999999999,1.3440000000000001,1.3444,1.3448,1.3451,1.3456999999999999,1.3460000000000001,1.3465,1.3468,1.3472999999999999,1.3476999999999999,1.3481000000000001,1.3485,1.349,1.3494999999999999,1.3499000000000001,1.3501000000000001,1.3505,1.3511,1.3513999999999999,1.3517999999999999,1.3521000000000001,1.3527,1.3531,1.3533999999999999,1.3541000000000001,1.3544,1.3548,1.355,1.3556999999999999,1.3561000000000001,1.3563000000000001,1.3566,1.3573999999999999,1.3575999999999999,1.3579000000000001,1.3584000000000001,1.3587,1.3592,1.3594999999999999,1.3600000000000001,1.3603000000000001,1.3608,1.3611,1.3614999999999999,1.3617999999999999,1.3623000000000001,1.3628,1.3631,1.3633999999999999,1.3638999999999999,1.3644000000000001,1.3647,1.365]],"yo":[[0.48999999999999999,0.71999999999999997,0.76000000000000001,0.79000000000000004,0.81999999999999995,0.83999999999999997,0.85999999999999999,0.88,0.91000000000000003,0.93999999999999995,0.96999999999999997,0.98999999999999999,1.01,1.05,1.0800000000000001,1.1100000000000001,1.1399999999999999,1.1599999999999999,1.21,1.25,1.29,1.3300000000000001,1.3600000000000001,1.3799999999999999,1.4299999999999999,1.48,1.51,1.55,1.5800000000000001,1.6499999999999999,1.7,1.76,1.8,1.8400000000000001,1.8799999999999999,1.9399999999999999,1.99,2.0299999999999998,2.0699999999999998,2.1099999999999999,2.1600000000000001,2.2000000000000002,2.2400000000000002,2.27,2.3100000000000001,2.3399999999999999,2.3700000000000001,2.3999999999999999,2.4199999999999999,2.4500000000000002,2.4700000000000002,2.52,2.5600000000000001,2.6000000000000001,2.6400000000000001,2.6699999999999999,2.7000000000000002,2.73,2.7599999999999998,2.7799999999999998,2.7999999999999998,2.8300000000000001,2.8500000000000001,2.8700000000000001,2.8900000000000001,2.9199999999999999,2.96,2.9900000000000002,3.02,3.04,3.0600000000000001,3.0899999999999999,3.1200000000000001,3.1400000000000001,3.1600000000000001,3.21,3.2400000000000002,3.2799999999999998,3.3100000000000001,3.3399999999999999,3.3700000000000001,3.3900000000000001,3.4199999999999999,3.4500000000000002,3.4700000000000002,3.5,3.52,3.54,3.5600000000000001,3.5800000000000001,3.6000000000000001,3.6200000000000001,3.6400000000000001,3.6600000000000001,3.6699999999999999,3.6899999999999999,3.71,3.7200000000000002,3.7400000000000002,3.7599999999999998,3.7799999999999998,3.79,3.7999999999999998,3.8100000000000001,3.8199999999999998,3.8399999999999999,3.8500000000000001,3.8700000000000001,3.8799999999999999,3.8999999999999999,3.9100000000000001,3.9300000000000002,3.9399999999999999,3.9500000000000002,3.96,3.9700000000000002,3.98,4,4.0099999999999998,4.0199999999999996,4.0300000000000002,4.04,4.0499999999999998,4.0599999999999996,4.0700000000000003,4.0800000000000001,4.0899999999999999,4.0999999999999996,4.1100000000000003,4.1200000000000001,4.1299999999999999,4.1399999999999997,4.1500000000000004,4.1600000000000001,4.1699999999999999,4.1799999999999997,4.1900000000000004,4.2000000000000002,4.21,4.2199999999999998,4.2300000000000004,4.2400000000000002,4.25,4.2599999999999998,4.2800000000000002,4.2999999999999998,4.3099999999999996,4.3300000000000001,4.3399999999999999,4.3499999999999996,4.3700000000000001,4.3799999999999999,4.3899999999999997,4.4000000000000004,4.4100000000000001,4.4199999999999999,4.4299999999999997,4.4400000000000004,4.4500000000000002,4.46,4.4699999999999998,4.4800000000000004,4.4900000000000002,4.5,4.5099999999999998,4.5300000000000002,4.54,4.5599999999999996,4.5700000000000003,4.5800000000000001,4.5999999999999996,4.6100000000000003,4.6200000000000001,4.6299999999999999,4.6399999999999997,4.6500000000000004,4.6699999999999999,4.6799999999999997,4.6900000000000004,4.7000000000000002,4.7400000000000002,4.75,4.7599999999999998,4.7699999999999996,4.7800000000000002,4.79,4.7999999999999998,4.8099999999999996,4.8200000000000003,4.8300000000000001,4.8399999999999999,4.8499999999999996,4.8600000000000003,4.8799999999999999,4.8899999999999997,4.9100000000000001,4.9199999999999999,4.9400000000000004,4.9500000000000002,4.96,4.9699999999999998,4.9900000000000002,5,5.0099999999999998,5.0199999999999996,5.0300000000000002,5.04,5.0499999999999998,5.0700000000000003,5.0800000000000001,5.0899999999999999,5.0999999999999996,5.1200000000000001,5.1299999999999999,5.1399999999999997,5.1500000000000004,5.1600000000000001,5.1699999999999999,5.1799999999999997,5.1900000000000004,5.2000000000000002,5.21,5.2199999999999998,5.2400000000000002],[1.96,2.0099999999999998,2.0600000000000001,2.1099999999999999,2.1600000000000001,2.21,2.2599999999999998,2.3100000000000001,2.3599999999999999,2.4100000000000001,2.46,2.5099999999999998,2.5600000000000001,2.6099999999999999,2.6600000000000001,2.71,2.7599999999999998,2.8100000000000001,2.8500000000000001,2.8999999999999999,2.9500000000000002,3,3.0499999999999998,3.1000000000000001,3.1499999999999999,3.2000000000000002,3.25,3.2999999999999998,3.3500000000000001,3.3999999999999999,3.4500000000000002,3.5,3.5499999999999998,3.6000000000000001,3.6499999999999999,3.7000000000000002,3.75,3.7999999999999998,3.8500000000000001,3.8999999999999999,3.9500000000000002,4,4.0499999999999998,4.0999999999999996,4.1500000000000004,4.2000000000000002,4.25,4.2999999999999998,4.3499999999999996,4.4000000000000004,4.4500000000000002,4.5,4.5499999999999998,4.5999999999999996,4.6500000000000004,4.7000000000000002,4.75,4.7999999999999998,4.8499999999999996,4.9000000000000004,4.9500000000000002,5,5.0499999999999998,5.0999999999999996,5.1500000000000004,5.2000000000000002,5.25,5.2999999999999998,5.3499999999999996,5.4000000000000004,5.4500000000000002,5.5,5.5499999999999998,5.5999999999999996,5.6500000000000004,5.7000000000000002,5.75,5.7999999999999998,5.8499999999999996,5.9000000000000004,5.9500000000000002,6,6.0499999999999998,6.0999999999999996,6.1500000000000004,6.2000000000000002,6.25,6.2999999999999998,6.3499999999999996,6.4000000000000004,6.4500000000000002,6.5,6.5499999999999998,6.5999999999999996,6.6500000000000004,6.7000000000000002,6.75,6.7999999999999998,6.8499999999999996,6.9000000000000004,6.9500000000000002,7,7.0499999999999998,7.0999999999999996,7.1500000000000004,7.2000000000000002,7.25,7.2999999999999998,7.3499999999999996,7.4000000000000004,7.4500000000000002,7.5,7.5499999999999998,7.5999999999999996,7.6500000000000004,7.7000000000000002,7.75,7.7999999999999998,7.8499999999999996,7.9000000000000004,7.9500000000000002,8,8.0500000000000007,8.0999999999999996,8.1500000000000004,8.1999999999999993,8.25,8.3000000000000007,8.3499999999999996,8.4000000000000004,8.4499999999999993,8.5,8.5500000000000007,8.5999999999999996,8.6500000000000004,8.6999999999999993,8.75,8.8000000000000007,8.8499999999999996,8.9000000000000004,8.9499999999999993,9,9.0500000000000007,9.0999999999999996,9.1500000000000004,9.1999999999999993,9.25,9.3000000000000007,9.3499999999999996,9.4000000000000004,9.4499999999999993,9.5,9.5500000000000007,9.5999999999999996,9.6500000000000004,9.6999999999999993,9.75,9.8000000000000007,9.8499999999999996,9.9000000000000004,9.9499999999999993,10,10.1,10.199999999999999,10.300000000000001,10.4,10.5,10.6,10.699999999999999,10.800000000000001,10.9,11,11.1,11.199999999999999,11.300000000000001,11.4,11.5,11.6,11.699999999999999,11.800000000000001,11.9,12,12.1,12.199999999999999,12.300000000000001,12.4,12.5,12.6,12.699999999999999,12.800000000000001,12.9,13,13.1,13.199999999999999,13.300000000000001,13.4,13.5,13.6,13.699999999999999,13.800000000000001,13.9,14,14.1,14.199999999999999,14.300000000000001,14.4,14.5,14.6,14.699999999999999,14.800000000000001,14.9,15,15.1,15.199999999999999,15.300000000000001,15.4,15.5,15.6,15.699999999999999,15.800000000000001,15.9,16,16.100000000000001,16.199999999999999,16.300000000000001,16.399999999999999,16.5,16.600000000000001,16.699999999999999,16.800000000000001,16.899999999999999,17,17.100000000000001,17.199999999999999,17.300000000000001,17.399999999999999,17.5,17.600000000000001,17.699999999999999,17.800000000000001,17.899999999999999,18,18.100000000000001,18.199999999999999,18.300000000000001,18.399999999999999,18.5,18.600000000000001,18.699999999999999,18.800000000000001,18.899999999999999,19,19.100000000000001,19.199999999999999,19.300000000000001,19.399999999999999,19.5,19.600000000000001,19.699999999999999,19.800000000000001,19.899999999999999,20,20.100000000000001,20.199999999999999,20.300000000000001,20.399999999999999,20.5,20.600000000000001,20.699999999999999,20.800000000000001,20.899999999999999,21,21.100000000000001,21.199999999999999,21.300000000000001,21.399999999999999,21.5,21.600000000000001,21.699999999999999,21.800000000000001,21.899999999999999,22,22.100000000000001,22.199999999999999,22.300000000000001,22.399999999999999,22.5,22.600000000000001,22.699999999999999,22.800000000000001,22.899999999999999,23,23.100000000000001,23.199999999999999,23.300000000000001,23.399999999999999,23.5,23.600000000000001,23.699999999999999,23.800000000000001,23.899999999999999,24,24.100000000000001,24.199999999999999,24.300000000000001,24.399999999999999,24.5,24.600000000000001,24.699999999999999,24.800000000000001,24.899999999999999,25,25.100000000000001,25.199999999999999,25.300000000000001,25.399999999999999,25.5,25.600000000000001,25.699999999999999,25.800000000000001,25.899999999999999,26,26.100000000000001,26.199999999999999,26.300000000000001,26.399999999999999,26.5,26.600000000000001,26.699999999999999,26.800000000000001,26.899999999999999,27,27.100000000000001,27.199999999999999,27.300000000000001,27.399999999999999,27.5,27.600000000000001,27.699999999999999,27.800000000000001,27.899999999999999,28,28.100000000000001,28.199999999999999,28.300000000000001,28.399999999999999,28.5,28.600000000000001,28.699999999999999,28.800000000000001,28.899999999999999,29,29.100000000000001,29.199999999999999,29.300000000000001,29.399999999999999,29.5,29.600000000000001,29.699999999999999,29.800000000000001,29.899999999999999,30,30.100000000000001,30.199999999999999,30.300000000000001,30.399999999999999,30.5,30.600000000000001,30.699999999999999,30.800000000000001,30.899999999999999,31,31.100000000000001,31.199999999999999,31.300000000000001,31.399999999999999,31.5,31.600000000000001,31.699999999999999,31.800000000000001,31.899999999999999,32,32.100000000000001,32.200000000000003,32.299999999999997,32.399999999999999,32.5,32.600000000000001,32.700000000000003,32.799999999999997,32.899999999999999,33,33.100000000000001,33.200000000000003,33.299999999999997,33.399999999999999,33.5,33.600000000000001,33.700000000000003,33.799999999999997,33.899999999999999,34,34.100000000000001,34.200000000000003,34.299999999999997,34.399999999999999,34.5,34.600000000000001,34.700000000000003,34.799999999999997,34.899999999999999,35,35.100000000000001,35.200000000000003,35.299999999999997,35.399999999999999,35.5,35.600000000000001,35.700000000000003,35.799999999999997,35.899999999999999,36,36.100000000000001,36.200000000000003,36.299999999999997,36.399999999999999,36.5,36.600000000000001,36.700000000000003,36.799999999999997,36.899999999999999,37,37.100000000000001,37.200000000000003,37.299999999999997,37.399999999999999,37.5,37.600000000000001,37.700000000000003,37.799999999999997,37.899999999999999,38,38.100000000000001,38.200000000000003,38.299999999999997,38.399999999999999,38.5,38.600000000000001,38.700000000000003,38.799999999999997,38.899999999999999,39,39.100000000000001,39.200000000000003,39.299999999999997,39.399999999999999,39.5,39.600000000000001,39.700000000000003,39.799999999999997,39.899999999999999,40,40.100000000000001,40.200000000000003,40.299999999999997,40.399999999999999,40.5,40.600000000000001,40.700000000000003,40.799999999999997,40.899999999999999,41,41.100000000000001,41.200000000000003,41.299999999999997,41.399999999999999,41.5,41.600000000000001,41.700000000000003,41.799999999999997,41.899999999999999,42,42.100000000000001,42.200000000000003,42.299999999999997,42.399999999999999,42.5,42.600000000000001,42.700000000000003,42.799999999999997,42.899999999999999,43,43.100000000000001,43.200000000000003,43.299999999999997,43.399999999999999,43.5,43.600000000000001,43.700000000000003,43.799999999999997,43.899999999999999,44,44.100000000000001,44.200000000000003,44.299999999999997,44.399999999999999,44.5,44.600000000000001,44.700000000000003,44.799999999999997,44.899999999999999,45,45.100000000000001,45.200000000000003,45.299999999999997,45.399999999999999,45.5,45.600000000000001,45.700000000000003,45.799999999999997,45.899999999999999,46,46.100000000000001,46.200000000000003,46.299999999999997,46.399999999999999,46.5,46.600000000000001,46.700000000000003,46.799999999999997,46.899999999999999,47,47.100000000000001,47.200000000000003,47.299999999999997,47.399999999999999,47.5,47.600000000000001,47.700000000000003,47.799999999999997,47.899999999999999,48,48.100000000000001,48.200000000000003,48.299999999999997,48.399999999999999,48.5,48.600000000000001,48.700000000000003,48.799999999999997,48.899999999999999,49,49.100000000000001,49.200000000000003,49.299999999999997,49.399999999999999,49.5,49.600000000000001,49.700000000000003,49.799999999999997,49.899999999999999,50],[2.4300000000000002,2.48,2.5499999999999998,2.6000000000000001,2.6499999999999999,2.7000000000000002,2.75,2.7999999999999998,2.8500000000000001,2.8999999999999999,2.9500000000000002,3,3.0499999999999998,3.1000000000000001,3.1499999999999999,3.2000000000000002,3.25,3.2999999999999998,3.3500000000000001,3.3999999999999999,3.4500000000000002,3.5,3.5499999999999998,3.6000000000000001,3.6499999999999999,3.7000000000000002,3.75,3.7999999999999998,3.8500000000000001,3.8999999999999999,3.9500000000000002,4,4.0499999999999998,4.0999999999999996,4.1500000000000004,4.2000000000000002,4.25,4.2999999999999998,4.3499999999999996,4.4000000000000004,4.4500000000000002,4.5,4.5499999999999998,4.5999999999999996,4.6500000000000004,4.7000000000000002,4.75,4.7999999999999998,4.8499999999999996,4.9000000000000004,4.9500000000000002,5,5.0499999999999998,5.0999999999999996,5.1500000000000004,5.2000000000000002,5.25,5.2999999999999998,5.3499999999999996,5.4000000000000004,5.4500000000000002,5.5,5.5499999999999998,5.5999999999999996,5.6500000000000004,5.7000000000000002,5.75,5.7999999999999998,5.8499999999999996,5.9000000000000004,5.9500000000000002,6,6.0499999999999998,6.0999999999999996,6.1500000000000004,6.2000000000000002,6.25,6.2999999999999998,6.3499999999999996,6.4000000000000004,6.4500000000000002,6.5,6.5499999999999998,6.5999999999999996,6.6500000000000004,6.7000000000000002,6.75,6.7999999999999998,6.8499999999999996,6.9000000000000004,6.9500000000000002,7,7.0499999999999998,7.0999999999999996,7.1500000000000004,7.2000000000000002,7.25,7.2999999999999998,7.3499999999999996,7.4000000000000004,7.4500000000000002,7.5,7.5499999999999998,7.5999999999999996,7.6500000000000004,7.7000000000000002,7.75,7.7999999999999998,7.8499999999999996,7.9000000000000004,7.9500000000000002,8,8.0500000000000007,8.0999999999999996,8.1500000000000004,8.1999999999999993,8.25,8.3000000000000007,8.3499999999999996,8.4000000000000004,8.4499999999999993,8.5,8.5500000000000007,8.5999999999999996,8.6500000000000004,8.6999999999999993,8.75,8.8000000000000007,8.8499999999999996,8.9000000000000004,8.9499999999999993,9,9.0500000000000007,9.0999999999999996,9.1500000000000004,9.1999999999999993,9.25,9.3000000000000007,9.3499999999999996,9.4000000000000004,9.4499999999999993,9.5,9.5500000000000007,9.5999999999999996,9.6500000000000004,9.6999999999999993,9.75,9.8000000000000007,9.8499999999999996,9.9000000000000004,9.9499999999999993,10,10.050000000000001,10.1,10.15,10.199999999999999,10.25,10.300000000000001,10.35,10.4,10.449999999999999,10.5,10.550000000000001,10.6,10.65,10.699999999999999,10.75,10.800000000000001,10.85,10.9,10.949999999999999,11,11.050000000000001,11.1,11.15,11.199999999999999,11.25,11.300000000000001,11.35,11.4,11.449999999999999,11.5,11.550000000000001,11.6,11.65,11.699999999999999,11.75,11.800000000000001,11.85,11.9,11.949999999999999,12,12.050000000000001,12.1,12.15,12.199999999999999,12.25,12.300000000000001,12.35,12.4,12.449999999999999,12.5,12.550000000000001,12.6,12.65,12.699999999999999,12.75,12.800000000000001,12.85,12.9,12.949999999999999,13,13.050000000000001,13.1,13.15,13.199999999999999,13.25,13.300000000000001,13.35,13.4,13.449999999999999,13.5,13.550000000000001,13.6,13.65,13.699999999999999,13.75,13.800000000000001,13.85,13.9,13.949999999999999,14,14.050000000000001,14.1,14.15,14.199999999999999,14.25,14.300000000000001,14.35,14.4,14.449999999999999,14.5,14.550000000000001,14.6,14.65,14.699999999999999,14.75,14.800000000000001,14.85,14.9,14.949999999999999,15,15.050000000000001,15.1,15.15,15.199999999999999,15.25,15.300000000000001,15.35,15.4,15.449999999999999,15.5,15.550000000000001,15.6,15.65,15.699999999999999,15.75,15.800000000000001,15.85,15.9,15.949999999999999,16,16.050000000000001,16.100000000000001,16.149999999999999,16.199999999999999,16.25,16.300000000000001,16.350000000000001,16.399999999999999,16.449999999999999,16.5,16.550000000000001,16.600000000000001,16.649999999999999,16.699999999999999,16.75,16.800000000000001,16.850000000000001,16.899999999999999,16.949999999999999,17,17.050000000000001,17.100000000000001,17.149999999999999,17.199999999999999,17.25,17.300000000000001,17.350000000000001,17.399999999999999,17.449999999999999,17.5,17.550000000000001,17.600000000000001,17.649999999999999,17.699999999999999,17.75,17.800000000000001,17.850000000000001,17.899999999999999,17.949999999999999,18,18.050000000000001,18.100000000000001,18.149999999999999,18.199999999999999,18.25,18.300000000000001,18.350000000000001,18.399999999999999,18.449999999999999,18.5,18.550000000000001,18.600000000000001,18.649999999999999,18.699999999999999,18.75,18.800000000000001,18.850000000000001,18.899999999999999,18.949999999999999,19,19.050000000000001,19.100000000000001,19.149999999999999,19.199999999999999,19.25,19.300000000000001,19.350000000000001,19.399999999999999,19.449999999999999,19.5,19.550000000000001,19.600000000000001,19.649999999999999,19.699999999999999,19.75,19.800000000000001,19.850000000000001,19.899999999999999,19.949999999999999,20,20.050000000000001,20.100000000000001,20.149999999999999,20.199999999999999,20.25,20.300000000000001,20.350000000000001,20.399999999999999,20.449999999999999,20.5,20.550000000000001,20.600000000000001,20.649999999999999,20.699999999999999,20.75,20.800000000000001,20.850000000000001,20.899999999999999,20.949999999999999,21,21.050000000000001,21.100000000000001,21.149999999999999,21.199999999999999,21.25,21.300000000000001,21.350000000000001,21.399999999999999,21.449999999999999,21.5,21.550000000000001,21.600000000000001,21.649999999999999,21.699999999999999,21.75,21.800000000000001,21.850000000000001,21.899999999999999,21.949999999999999,22,22.050000000000001,22.100000000000001,22.149999999999999,22.199999999999999,22.25,22.300000000000001,22.350000000000001,22.399999999999999,22.449999999999999,22.5,22.550000000000001,22.600000000000001,22.649999999999999,22.699999999999999,22.75,22.800000000000001,22.850000000000001,22.899999999999999,22.949999999999999,23,23.050000000000001,23.100000000000001,23.149999999999999,23.199999999999999,23.25,23.300000000000001,23.350000000000001,23.399999999999999,23.449999999999999,23.5,23.550000000000001,23.600000000000001,23.649999999999999,23.699999999999999,23.75,23.800000000000001,23.850000000000001,23.899999999999999,23.949999999999999,24,24.050000000000001,24.100000000000001,24.149999999999999,24.199999999999999,24.25,24.300000000000001,24.350000000000001,24.399999999999999,24.449999999999999,24.5,24.550000000000001,24.600000000000001,24.649999999999999,24.699999999999999,24.75,24.800000000000001,24.850000000000001,24.899999999999999,24.949999999999999,25,25.050000000000001,25.100000000000001,25.149999999999999,25.199999999999999,25.25,25.300000000000001,25.350000000000001,25.399999999999999,25.449999999999999,25.5,25.550000000000001,25.600000000000001,25.649999999999999,25.699999999999999,25.75,25.800000000000001,25.850000000000001,25.899999999999999,25.949999999999999,26,26.050000000000001,26.100000000000001,26.149999999999999,26.199999999999999,26.25,26.300000000000001,26.350000000000001,26.399999999999999,26.449999999999999,26.5,26.550000000000001,26.600000000000001,26.649999999999999,26.699999999999999,26.75,26.800000000000001,26.850000000000001,26.899999999999999,26.949999999999999,27,27.050000000000001,27.100000000000001,27.149999999999999,27.199999999999999,27.25,27.300000000000001,27.350000000000001,27.399999999999999,27.449999999999999,27.5,27.550000000000001,27.600000000000001,27.649999999999999,27.699999999999999,27.75,27.800000000000001,27.850000000000001,27.899999999999999,27.949999999999999,28,28.050000000000001,28.100000000000001,28.149999999999999,28.199999999999999,28.25,28.300000000000001,28.350000000000001,28.399999999999999,28.449999999999999,28.5,28.550000000000001,28.600000000000001,28.649999999999999,28.699999999999999,28.75,28.800000000000001,28.850000000000001,28.899999999999999,28.949999999999999,29,29.050000000000001,29.100000000000001,29.149999999999999,29.199999999999999,29.25,29.300000000000001,29.350000000000001,29.399999999999999,29.449999999999999,29.5,29.550000000000001,29.600000000000001,29.649999999999999,29.699999999999999,29.75,29.800000000000001,29.850000000000001,29.899999999999999,29.949999999999999,30,30.050000000000001,30.100000000000001,30.149999999999999,30.199999999999999,30.25,30.300000000000001,30.350000000000001,30.399999999999999,30.449999999999999,30.5,30.550000000000001,30.600000000000001,30.649999999999999,30.699999999999999,30.75,30.800000000000001,30.850000000000001,30.899999999999999,30.949999999999999,31,31.050000000000001,31.100000000000001,31.149999999999999,31.199999999999999,31.25,31.300000000000001,31.350000000000001,31.399999999999999,31.449999999999999,31.5,31.550000000000001,31.600000000000001,31.649999999999999,31.699999999999999,31.75,31.800000000000001,31.850000000000001,31.899999999999999,31.949999999999999,32,32.049999999999997,32.100000000000001,32.149999999999999,32.200000000000003,32.25,32.299999999999997,32.350000000000001,32.399999999999999,32.450000000000003,32.5,32.549999999999997,32.600000000000001,32.649999999999999,32.700000000000003,32.75,32.799999999999997,32.850000000000001,32.899999999999999,32.950000000000003,33,33.049999999999997,33.100000000000001,33.149999999999999,33.200000000000003,33.25,33.299999999999997,33.350000000000001,33.399999999999999,33.450000000000003,33.5,33.549999999999997,33.600000000000001,33.649999999999999,33.700000000000003,33.75,33.799999999999997,33.850000000000001,33.899999999999999,33.950000000000003,34,34.049999999999997,34.100000000000001,34.149999999999999,34.200000000000003,34.25,34.299999999999997,34.350000000000001,34.399999999999999,34.450000000000003,34.5,34.549999999999997,34.600000000000001,34.649999999999999,34.700000000000003,34.75,34.799999999999997,34.850000000000001,34.899999999999999,34.950000000000003,35,35.049999999999997,35.100000000000001,35.149999999999999,35.200000000000003,35.25,35.299999999999997,35.350000000000001,35.399999999999999,35.450000000000003,35.5,35.549999999999997,35.600000000000001,35.649999999999999,35.700000000000003,35.75,35.799999999999997,35.850000000000001,35.899999999999999,35.950000000000003,36,36.049999999999997,36.100000000000001,36.149999999999999,36.200000000000003,36.25,36.299999999999997,36.350000000000001,36.399999999999999,36.450000000000003,36.5,36.549999999999997,36.600000000000001,36.649999999999999,36.700000000000003,36.75,36.799999999999997,36.850000000000001,36.899999999999999,36.950000000000003,37,37.049999999999997,37.100000000000001,37.149999999999999,37.200000000000003,37.25,37.299999999999997,37.350000000000001,37.399999999999999,37.450000000000003,37.5,37.549999999999997,37.600000000000001,37.649999999999999,37.700000000000003,37.75,37.799999999999997,37.850000000000001,37.899999999999999,37.950000000000003,38,38.049999999999997,38.100000000000001,38.149999999999999,38.200000000000003,38.25,38.299999999999997,38.350000000000001,38.399999999999999,38.450000000000003,38.5,38.549999999999997,38.600000000000001,38.649999999999999,38.700000000000003,38.75,38.799999999999997,38.850000000000001,38.899999999999999,38.950000000000003,39,39.049999999999997,39.100000000000001,39.149999999999999,39.200000000000003,39.25,39.299999999999997,39.350000000000001,39.399999999999999,39.450000000000003,39.5,39.549999999999997,39.600000000000001,39.649999999999999,39.700000000000003,39.75,39.799999999999997,39.850000000000001,39.899999999999999,39.950000000000003,40,40.049999999999997,40.100000000000001,40.149999999999999,40.200000000000003,40.25,40.299999999999997,40.350000000000001,40.399999999999999,40.450000000000003,40.5,40.549999999999997,40.600000000000001,40.649999999999999,40.700000000000003,40.75,40.799999999999997,40.850000000000001,40.899999999999999,40.950000000000003,41,41.049999999999997,41.100000000000001,41.149999999999999,41.200000000000003,41.25,41.299999999999997,41.350000000000001,41.399999999999999,41.450000000000003,41.5,41.549999999999997,41.600000000000001,41.649999999999999,41.700000000000003,41.75,41.799999999999997,41.850000000000001,41.899999999999999,41.950000000000003,42,42.049999999999997,42.100000000000001,42.149999999999999,42.200000000000003,42.25,42.299999999999997,42.350000000000001,42.399999999999999,42.450000000000003,42.5,42.549999999999997,42.600000000000001,42.649999999999999,42.700000000000003,42.75,42.799999999999997,42.850000000000001,42.899999999999999,42.950000000000003,43,43.049999999999997,43.100000000000001,43.149999999999999,43.200000000000003,43.25,43.299999999999997,43.350000000000001,43.399999999999999,43.450000000000003,43.5,43.549999999999997,43.600000000000001,43.649999999999999,43.700000000000003,43.75,43.799999999999997,43.850000000000001,43.899999999999999,43.950000000000003,44,44.049999999999997,44.100000000000001,44.149999999999999,44.200000000000003,44.25,44.299999999999997,44.350000000000001,44.399999999999999,44.450000000000003,44.5,44.549999999999997,44.600000000000001,44.649999999999999,44.700000000000003,44.75,44.799999999999997,44.850000000000001,44.899999999999999,44.950000000000003,45,45.049999999999997,45.100000000000001,45.149999999999999,45.200000000000003,45.25,45.299999999999997,45.350000000000001,45.399999999999999,45.450000000000003,45.5,45.549999999999997,45.600000000000001,45.649999999999999,45.700000000000003,45.75,45.799999999999997,45.850000000000001,45.899999999999999,45.950000000000003,46,46.049999999999997,46.100000000000001,46.149999999999999,46.200000000000003,46.25,46.299999999999997,46.350000000000001,46.399999999999999,46.450000000000003,46.5,46.549999999999997,46.600000000000001,46.649999999999999,46.700000000000003,46.75,46.799999999999997,46.850000000000001,46.899999999999999,46.950000000000003,47,47.049999999999997,47.100000000000001,47.149999999999999,47.200000000000003,47.25,47.299999999999997,47.350000000000001,47.399999999999999,47.450000000000003,47.5,47.549999999999997,47.600000000000001,47.649999999999999,47.700000000000003,47.75,47.799999999999997,47.850000000000001,47.899999999999999,47.950000000000003,48,48.049999999999997,48.100000000000001,48.149999999999999,48.200000000000003,48.25,48.299999999999997,48.350000000000001,48.399999999999999,48.450000000000003,48.5,48.549999999999997,48.600000000000001,48.649999999999999,48.700000000000003,48.75,48.799999999999997,48.850000000000001,48.899999999999999,48.950000000000003,49,49.049999999999997,49.100000000000001,49.149999999999999,49.200000000000003,49.25,49.299999999999997,49.350000000000001,49.399999999999999,49.450000000000003,49.5,49.549999999999997,49.600000000000001,49.649999999999999,49.700000000000003,49.75,49.799999999999997,49.850000000000001,49.899999999999999,49.950000000000003,50]],"z":[{"value":15,"unit":"MPa","name":"","comment":null,"realZ":15},{"value":20,"unit":"MPa","name":"","comment":null,"realZ":20},{"value":25,"unit":"MPa","name":"","comment":null,"realZ":25}],"zo":[{"value":15,"unit":"MPa","name":"","comment":null,"realZ":15},{"value":20,"unit":"MPa","name":"","comment":null,"realZ":20},{"value":25,"unit":"MPa","name":"","comment":null,"realZ":25}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"creep-curve-90-\u00b0c-delrin\u00ae-100p-nc010.png","svgname":"creep-curve-90-\u00b0c-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","",""],"xmarker":[],"option":1},"moist":0,"name":"Creep curve 90\u00b0C","shortname":"Creep"},{"id":17,"addId":[],"data":{"name":"Specific volume-temperature (pvT) ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Temperature in","unit":"\u00b0C","log":false},"y":{"name":"Spec. volume in","unit":"E-3 m\u00b3\/kg","log":false},"z":{"name":"","unit":"MPa"}},"x":[[20,40,60,80,100,120,140,160,180,200],[20,40,60,80,100,120,140,160,180,200],[20,40,60,80,100,120,140,160,180,200],[20,40,60,80,100,120,140,160,180,200]],"y":[[0.70499999999999996,0.71099999999999997,0.71799999999999997,0.72699999999999998,0.74099999999999999,0.76500000000000001,0.81299999999999994,0.83599999999999997,0.84499999999999997,0.85499999999999998],[0.69899999999999995,0.70499999999999996,0.71099999999999997,0.71999999999999997,0.73199999999999998,0.753,0.79300000000000004,0.81999999999999995,0.82799999999999996,0.83599999999999997],[0.68799999999999994,0.69399999999999995,0.69999999999999996,0.70699999999999996,0.71699999999999997,0.73299999999999998,0.76200000000000001,0.79600000000000004,0.80200000000000005,0.80800000000000005],[0.67900000000000005,0.68400000000000005,0.68999999999999995,0.69699999999999995,0.70499999999999996,0.71699999999999997,0.73799999999999999,0.77800000000000002,0.78300000000000003,0.78800000000000003]],"xo":null,"yo":null,"z":[{"value":0.10000000000000001,"unit":"MPa","name":"","comment":null,"realZ":0.10000000000000001},{"value":40,"unit":"MPa","name":"","comment":null,"realZ":40},{"value":120,"unit":"MPa","name":"","comment":null,"realZ":120},{"value":200,"unit":"MPa","name":"","comment":null,"realZ":200}],"zo":[{"value":0.10000000000000001,"unit":"MPa","name":"","comment":null,"realZ":0.10000000000000001},{"value":40,"unit":"MPa","name":"","comment":null,"realZ":40},{"value":120,"unit":"MPa","name":"","comment":null,"realZ":120},{"value":200,"unit":"MPa","name":"","comment":null,"realZ":200}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"specific-volume-temperature-pvt-delrin\u00ae-100p-nc010.png","svgname":"specific-volume-temperature-pvt-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":["","","",""],"xmarker":[],"option":1},"moist":0,"name":"Specific volume-temperature (pvT)","shortname":"pvT"},{"id":22,"addId":[],"data":{"name":"Tensile modulus-temperature ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Temperature in","unit":"\u00b0C","log":false},"y":{"name":"Tensile modulus in","unit":"MPa","log":true},"z":{"name":"","unit":""}},"x":[[-40,-37.681159420289852,-35.362318840579704,-33.043478260869556,-30.724637681159411,-28.405797101449267,-26.086956521739122,-23.768115942028977,-21.449275362318833,-19.130434782608688,-16.811594202898544,-14.492753623188399,-12.173913043478255,-9.85507246376811,-7.5362318840579654,-5.2173913043478208,-2.8985507246376758,-0.57971014492753081,1.7391304347826142,4.0579710144927592,6.3768115942029038,8.6956521739130483,11.014492753623193,13.333333333333337,15.652173913043482,17.971014492753628,20.289855072463773,22.608695652173918,24.927536231884062,27.246376811594207,29.565217391304351,31.884057971014496,34.20289855072464,36.521739130434788,38.840579710144937,41.159420289855085,43.478260869565233,45.797101449275381,48.115942028985529,50.434782608695677,52.753623188405825,55.072463768115973,57.391304347826122,59.71014492753627,62.028985507246418,64.347826086956559,66.6666666666667,68.985507246376841,71.304347826086982,73.623188405797123,75.942028985507264,78.260869565217405,80.579710144927546,82.898550724637687,85.217391304347828,87.536231884057969,89.85507246376811,92.173913043478251,94.492753623188392,96.811594202898533,99.130434782608674,101.44927536231882,103.76811594202896,106.0869565217391,108.40579710144924,110.72463768115938,113.04347826086952,115.36231884057966,117.6811594202898,119.99999999999994]],"y":[[3621.0000000000005,3570.8363854682757,3521.6092824042116,3473.5373437241719,3426.8267661450673,3381.6721137943036,3338.2572554607955,3296.7564039161016,3257.3352474950466,3220.1521660243816,3185.3595252085292,3153.1050457123288,3123.5332454179511,3096.7869556799569,3073.0089148701259,3052.343445110906,3034.9382208709426,3020.9461410752192,3010.4690310878577,3003.1124582999801,2998.2358346325859,2995.2077447793713,2993.4035934628878,2992.2024137262929,2990.9849742345177,2989.1331720239764,2986.0307043937869,2981.0650134495181,2973.6184671644914,2963.0048220666758,2948.5239611434631,2929.5034558446241,2905.3086558736227,2875.3539392746584,2839.1149391805129,2796.1413918273565,2746.0701801774435,2688.6380826471564,2623.6936823478845,2551.2078545621121,2471.2822345201134,2384.1550790795559,2290.2039788559305,2189.9449544496256,2084.2778125958389,1975.5584501430794,1866.3571117951383,1758.8510313519732,1654.8235161446667,1555.6843733962892,1462.5049310562365,1376.0623045043797,1296.8884765134762,1225.3207946703071,1161.5515286151228,1105.6750933495398,1057.7323981839088,1017.5738470666764,984.26598240911551,956.79539682081713,934.30650434375684,916.06647843677979,901.43738414028928,889.85393260672345,880.8056649416942,873.82269668175786,868.46439873082352,864.31057565018807,860.95484186419981,857.99999999999966]],"xo":[[-40,0,23,60,90,120]],"yo":[[3621,3018,2980,2177,1055,858]],"z":[{"value":null,"unit":"","name":"","comment":null,"realZ":null}],"zo":[{"value":null,"unit":"","name":"","comment":null,"realZ":null}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"tensile-modulus-temperature-delrin\u00ae-100p-nc010.png","svgname":"tensile-modulus-temperature-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":[""],"xmarker":[],"option":1},"moist":0,"name":"Tensile modulus-temperature","shortname":"E T"},{"id":112,"addId":[],"data":{"name":"Tensile Fatigue, 10Hz, R=0.1 ","name2":"Delrin\u00ae 100P NC010","nameRef":null,"moist":0,"orientation":"L","axes":{"x":{"name":"Cycles","unit":"","log":true},"y":{"name":"Stress in","unit":"MPa","log":false},"z":{"name":"","unit":"\u00b0C"}},"x":[[1800,6830,7670,13800,2000000]],"y":[[42.600000000000001,39.899999999999999,39.700000000000003,38.200000000000003,37.299999999999997]],"xo":null,"yo":null,"z":[{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23}],"zo":[{"value":23,"unit":"\u00b0C","name":"","comment":null,"realZ":23}],"keys":[],"comment":"","standardcomment":null,"watermark":"October 2026","styles":{"font":"diodrum","font-size":"1em","watermark":{"fill":"#969696","font-size":"0.8em"},"comment":{"font-size":"0.8em"},"legend":{"border":{"stroke":"black","stroke-width":"1px","fill":"none"}}},"config":{"orientation":"L","width":800,"height":600,"gridsize":0,"thumbnail":false,"zoom":true,"tooltip":true,"restricted":false,"target":"","stroke":["width=>2"],"axes":{"x":{"subticks":false},"y":{"subticks":false}},"switchColors":[],"copyColors":[],"curvepoints":{"show":false,"color":"curve","fill":1,"radius":3},"copy":{"scale":1},"legend":{"showcurvepoints":false,"border":{"enable":false,"offset":10,"paddingx":4}},"download":{"scale":1,"name":"tensile-fatigue-10hz-r-0.1-delrin\u00ae-100p-nc010.png","svgname":"tensile-fatigue-10hz-r-0.1-delrin\u00ae-100p-nc010.svg","type":"svg+png"},"clipboard":{"serverUrl":"https:\/\/delrin.materialdatacenter.com\/api\/v1\/mchart","filenamelength":20,"width":800,"height":600},"watermark":{"position":"fixed","x":10,"y":20},"titlebar":{"repositiontitle":false,"offsetlogo":20,"logoRight":true,"innerColor":"rgb(255,255,255)","outsideColor":"rgb(255,255,255)","logo":"data:image\/svg+xml;base64,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","logoWidth":350,"logoHeight":150,"padding":{"top":10},"yoffsettitle":15}},"add":[""],"xmarker":[],"option":1},"moist":0,"name":"Tensile Fatigue, 10Hz, R=0.1 @ mm","shortname":"Fatigue"}],"name":"Diagrams","pos":20,"type":"Mpt"}],"general":{"name":"Delrin\u00ae 100P NC010","abbt":"POM","pname":"Delrin","pshortname":"Delrin","pid":52,"region":[],"assortment_name":"ACETAL RESIN","assortment_color":"","lastchange":"2026-02-06","prod_status":"current","moisturedep":0},"id":"11804","injds":true,"psds":false,"bmds":false,"extrds":true,"eqds":true,"ris":true,"sdsurl":1,"dialinks":[]}